  "name": "Binder jetting stage parameters reported in two metal studies",
  "description": "Compares printing, curing or drying, sintering and density parameters for binder-jetted H13 tool steel (Widomski et al., Materials 2025) and alloy 625 from water- and gas-atomised powders (Mostafaei et al., Data in Brief 2016). Values are as reported by each study for its own material and machine, and are not general settings.",
  "page": "https://casrai.org/guides/binder-jetting",
  "publisher": "CASRAI",
  "license": "https://creativecommons.org/licenses/by/4.0/",
  "dateModified": "2026-11-14T15:19:25Z",
  "temporalCoverage": null,
  "spatialCoverage": null,
  "columns": [
    {
      "name": "Study case",
      "unit": "",
      "description": ""
    },
    {
      "name": "Layer thickness",
      "unit": "um",
      "description": ""
    },
    {
      "name": "Drying or curing temperature",
      "unit": "degC",
      "description": ""
    },
    {
      "name": "Sintering temperature",
      "unit": "degC",
      "description": ""
    },
    {
      "name": "Sintering hold time",
      "unit": "h",
      "description": ""
    },
    {
      "name": "Sintering atmosphere",
      "unit": "",
      "description": ""
    },
    {
      "name": "Highest relative density reported",
      "unit": "%",
      "description": ""
    }
  ],
  "rows": [
    {
      "Study case": "H13 tool steel (Widomski et al. 2025)",
      "Layer thickness": 70,
      "Drying or curing temperature": 35,
      "Sintering temperature": 1310,
      "Sintering hold time": 4,
      "Sintering atmosphere": "Argon",
      "Highest relative density reported": 99.3
    },
    {
      "Study case": "Alloy 625, water-atomised powder (Mostafaei et al. 2016)",
      "Layer thickness": 100,
      "Drying or curing temperature": 175,
      "Sintering temperature": 1270,
      "Sintering hold time": 4,
      "Sintering atmosphere": "Vacuum",
      "Highest relative density reported": 95
    },
    {
      "Study case": "Alloy 625, gas-atomised powder (Mostafaei et al. 2016)",
      "Layer thickness": 100,
      "Drying or curing temperature": 175,
      "Sintering temperature": 1285,
      "Sintering hold time": 4,
      "Sintering atmosphere": "Vacuum",
      "Highest relative density reported": 99.2
    }
  ],
  "sources": [
    {
      "title": "Widomski et al., Comparative Study of Different Additive Manufacturing Methods for H13 Tool Steel",
      "url": "https://pmc.ncbi.nlm.nih.gov/articles/PMC12692884/",
      "accessed": "2026-11-14"
    },
    {
      "title": "Mostafaei et al., alloy 625 water- vs gas-atomized powders, Data in Brief 10",
      "url": "https://pmc.ncbi.nlm.nih.gov/articles/PMC5144650/",
      "accessed": "2026-11-14"
    }
  ]
}