  "name": "Factors reported to affect degradation rate of polylactide and related polymers",
  "description": "Compiled from Lyu and Untereker (2009), a review of degradability of polymers for implantable biomedical devices: each rate factor with the effect the review reports, as a checklist of parameters to record when specifying a degradable polymer.",
  "page": "https://casrai.org/guides/biodegradable-polymers",
  "publisher": "CASRAI",
  "license": "https://creativecommons.org/licenses/by/4.0/",
  "dateModified": "2026-11-14T15:31:33Z",
  "temporalCoverage": null,
  "spatialCoverage": null,
  "columns": [
    {
      "name": "Factor",
      "unit": "",
      "description": ""
    },
    {
      "name": "Reported effect or note",
      "unit": "",
      "description": ""
    },
    {
      "name": "Degradation mechanism affected",
      "unit": "",
      "description": ""
    }
  ],
  "rows": [
    {
      "Factor": "Bond chemistry",
      "Reported effect or note": "Ester and anhydride bonds react more readily with water; conjugation and bulky side groups slow hydrolysis",
      "Degradation mechanism affected": "Hydrolysis"
    },
    {
      "Factor": "Water uptake",
      "Reported effect or note": "Hydrolysis depends on water concentration; about 1 wt% uptake reported for polylactide",
      "Degradation mechanism affected": "Hydrolysis"
    },
    {
      "Factor": "pH",
      "Reported effect or note": "Little effect on solid polylactide because ions barely penetrate; slowest at pH 4 in solution",
      "Degradation mechanism affected": "Hydrolysis"
    },
    {
      "Factor": "Molecular weight",
      "Reported effect or note": "Chain-end acids autocatalyze hydrolysis; matters more at low molecular weight",
      "Degradation mechanism affected": "Hydrolysis"
    },
    {
      "Factor": "Monomer sequence",
      "Reported effect or note": "More L-D linkages in polylactide degraded faster",
      "Degradation mechanism affected": "Hydrolysis"
    },
    {
      "Factor": "Thickness",
      "Reported effect or note": "Thick samples tend towards surface erosion, thin samples towards bulk degradation",
      "Degradation mechanism affected": "Hydrolysis"
    },
    {
      "Factor": "Oxidant exposure",
      "Reported effect or note": "Oxidants from inflammatory cells cause free-radical chain scission; polyethylene, vinyl polymers and polyether polyurethanes susceptible",
      "Degradation mechanism affected": "Oxidation"
    }
  ],
  "sources": [
    {
      "title": "Lyu S, Untereker D. Degradability of Polymers for Implantable Biomedical Devices. Int J Mol Sci 2009",
      "url": "https://pmc.ncbi.nlm.nih.gov/articles/PMC2769140",
      "accessed": "2026-11-14"
    }
  ]
}