  "name": "ACI 318-19(22) exposure classes: maximum w/cm, minimum f'c and added requirements",
  "description": "Compiled by CASRAI from Obla and Lobo's 2023 Concrete International guide to selecting ACI 318-19(22) exposure classes. For each F, S, W and C class it lists the exposure condition, maximum water-cementitious materials ratio, minimum specified compressive strength and the main added requirement. Chloride limits are water-soluble chloride ion as percent by mass of cementitious material.",
  "page": "https://casrai.org/guides/concrete-durability",
  "publisher": "CASRAI",
  "license": "https://creativecommons.org/licenses/by/4.0/",
  "dateModified": "2026-11-19T08:33:50Z",
  "temporalCoverage": "ACI CODE-318-19(22)",
  "spatialCoverage": null,
  "columns": [
    {
      "name": "Exposure class",
      "unit": "",
      "description": ""
    },
    {
      "name": "Category",
      "unit": "",
      "description": ""
    },
    {
      "name": "Exposure condition",
      "unit": "",
      "description": ""
    },
    {
      "name": "Maximum w/cm",
      "unit": "",
      "description": ""
    },
    {
      "name": "Minimum f'c",
      "unit": "psi",
      "description": ""
    },
    {
      "name": "Added requirement",
      "unit": "",
      "description": ""
    }
  ],
  "rows": [
    {
      "Exposure class": "F0",
      "Category": "Freezing and thawing",
      "Exposure condition": "Not exposed to freezing-and-thawing cycles",
      "Maximum w/cm": "N/A",
      "Minimum f'c": 2500,
      "Added requirement": "None beyond baseline"
    },
    {
      "Exposure class": "F1",
      "Category": "Freezing and thawing",
      "Exposure condition": "Exposed to freezing and thawing with limited contact with water",
      "Maximum w/cm": 0.55,
      "Minimum f'c": 3500,
      "Added requirement": "Air content per Table 19.3.3.1"
    },
    {
      "Exposure class": "F2",
      "Category": "Freezing and thawing",
      "Exposure condition": "Exposed to freezing and thawing with frequent contact with water",
      "Maximum w/cm": 0.45,
      "Minimum f'c": 4500,
      "Added requirement": "Air content per Table 19.3.3.1"
    },
    {
      "Exposure class": "F3",
      "Category": "Freezing and thawing",
      "Exposure condition": "Exposed to freezing and thawing with frequent contact with water and deicing chemicals",
      "Maximum w/cm": 0.4,
      "Minimum f'c": 5000,
      "Added requirement": "Air content and SCM limits; plain concrete 0.45 and 4500 psi"
    },
    {
      "Exposure class": "S0",
      "Category": "Sulfate",
      "Exposure condition": "Water-soluble sulfate in soil below 0.10% by mass",
      "Maximum w/cm": "N/A",
      "Minimum f'c": 2500,
      "Added requirement": "None beyond baseline"
    },
    {
      "Exposure class": "S1",
      "Category": "Sulfate",
      "Exposure condition": "Soil sulfate 0.10% to below 0.20%, or seawater",
      "Maximum w/cm": 0.5,
      "Minimum f'c": 4000,
      "Added requirement": "ASTM C150 Type II cement"
    },
    {
      "Exposure class": "S2",
      "Category": "Sulfate",
      "Exposure condition": "Soil sulfate 0.20% to below 2.00%",
      "Maximum w/cm": 0.45,
      "Minimum f'c": 4500,
      "Added requirement": "ASTM C150 Type V cement; no calcium chloride admixture"
    },
    {
      "Exposure class": "S3",
      "Category": "Sulfate",
      "Exposure condition": "Soil sulfate above 2.00%",
      "Maximum w/cm": "0.45 (option 1) or 0.40 (option 2)",
      "Minimum f'c": "4500 (option 1) or 5000 (option 2)",
      "Added requirement": "Type V cement; option 1 adds pozzolan or slag; no calcium chloride admixture"
    },
    {
      "Exposure class": "W0",
      "Category": "Water contact",
      "Exposure condition": "Dry in service",
      "Maximum w/cm": "N/A",
      "Minimum f'c": 2500,
      "Added requirement": "None beyond baseline"
    },
    {
      "Exposure class": "W1",
      "Category": "Water contact",
      "Exposure condition": "In contact with water where low permeability is not required",
      "Maximum w/cm": "N/A",
      "Minimum f'c": 2500,
      "Added requirement": "ASR evidence or mitigation per Section 26.4.2.2(d)"
    },
    {
      "Exposure class": "W2",
      "Category": "Water contact",
      "Exposure condition": "In contact with water where low permeability is required",
      "Maximum w/cm": 0.5,
      "Minimum f'c": 4000,
      "Added requirement": "ASR evidence or mitigation per Section 26.4.2.2(d)"
    },
    {
      "Exposure class": "C0",
      "Category": "Reinforcement corrosion",
      "Exposure condition": "Dry or protected from moisture",
      "Maximum w/cm": "N/A",
      "Minimum f'c": 2500,
      "Added requirement": "Chloride ion limit 1.00% nonprestressed, 0.06% prestressed"
    },
    {
      "Exposure class": "C1",
      "Category": "Reinforcement corrosion",
      "Exposure condition": "Exposed to moisture, no external chlorides",
      "Maximum w/cm": "N/A",
      "Minimum f'c": 2500,
      "Added requirement": "Chloride ion limit 0.30% nonprestressed, 0.06% prestressed"
    },
    {
      "Exposure class": "C2",
      "Category": "Reinforcement corrosion",
      "Exposure condition": "Exposed to moisture and external chlorides",
      "Maximum w/cm": 0.4,
      "Minimum f'c": 5000,
      "Added requirement": "Chloride ion limit 0.15% nonprestressed, 0.06% prestressed; cover per Section 20.5"
    }
  ],
  "sources": [
    {
      "title": "Obla and Lobo, Selecting Exposure Classes and Requirements for Durability, Concrete International, May 2023 (NRMCA reprint)",
      "url": "https://www.nrmca.org/wp-content/uploads/NRMCA_GuideToSelectingExposureClasses.pdf",
      "accessed": "2026-11-19"
    }
  ]
}