Skip to main content
v2026.11,986 entries · CC-BY 4.0

Wood Preservation: Industrial Methods, Standards, and Testing Protocols

An authoritative guide to wood preservation covering AWPA Use Categories, chemical preservative classes, cellular treatability, and standardized testing.

Written and maintained by CASRAI Editorial Board

Published

On this page

Wood preservation is the industrial and scientific process of applying chemical biocides, barrier treatments, and thermal modifications to timber to confer long-term resistance against biological degradation caused by wood-decaying basidiomycete fungi, subterranean and drywood termites, wood-boring beetles, and marine organisms. By fundamentally altering the chemical environment of wood cellular lumens and cell walls, standardized preservation systems extend the structural service life of forest products from mere months in aggressive environments to multiple decades in critical civil, residential, and marine infrastructure.

Definition, Mechanisms, and Scope of Wood Preservation

Wood preservation represents a vital intersection of wood anatomy, organic chemistry, and materials engineering. Untreated sapwood of virtually all commercial timber species possesses inherent susceptibility to rapid biodeterioration when exposed to ambient moisture exceeding the fiber saturation point (approximately 28% to 30% moisture content). Under favorable temperature and oxygen conditions, wood-decay fungi secrete hydrolytic and oxidative enzymes—principally endoglucanases, cellobiohydrolases, and lignin peroxidases—that depolymerize structural cellulose, hemicellulose, and lignin matrices, causing severe structural mass loss and progressive strength failure.

The biological agents responsible for timber degradation fall into three distinct hazard groups: decay fungi, wood-boring insects, and marine borers. Decay fungi encompass brown-rot fungi, which rapidly break down structural carbohydrates while leaving modified brown lignin frameworks; white-rot fungi, which simultaneously degrade both lignin and polysaccharides to leave soft, bleached fibers; and soft-rot microfungi, which create microscopic cavities within secondary cell walls under excessive moisture or high-nitrogen conditions. Wood-boring insects, including subterranean termites (Reticulitermes species), drywood termites (Incisitermes species), and powderpost beetles (Lyctinae and Anobiidae), mechanically excavate tunnels and ingest structural polymers. In saline and brackish waters, marine borers such as shipworms (molluscan teredinids) and gribbles (crustacean Limnoria species) rapidly destroy untreated structural pilings through internal boring.

Within the broader academic discipline of forestry ecology, wood preservation functions as a primary conservation mechanism. By multiplying the functional service life of harvested timber by factors of five to twenty, chemical preservation drastically reduces the annual timber harvest volumes required to maintain infrastructure, mitigating harvest pressures on natural forest stands and stabilizing sequestered carbon stocks over extended technological lifespans. The technological scope of preservation encompasses non-pressure surface coatings, diffusion treatments, thermal modifications, and full-scale industrial vacuum-pressure impregnation cylinders.

Wood Anatomy and Treatability: Cellular Permeability and Refractory Species

The chemical treatability of any timber member is governed strictly by its microscopic cellular architecture, fluid flow pathways, and the anatomical distinction between sapwood and heartwood. In living trees, sapwood conducts water and mineral nutrients upward through open, fluid-permeable longitudinal cells, while heartwood represents physiologically inactive inner wood where secondary metabolic extractives—such as tannins, stilbenes, flavonoids, and resins—have encrusted cell walls and pit membranes. Consequently, while the sapwood of most coniferous and broadleaved species readily accepts chemical solutions, heartwood displays profound resistance to fluid penetration.

In softwood species, longitudinal fluid conduction relies on elongated tracheids interconnected by microscopic bordered pit pairs. During the commercial drying and seasoning that precedes preservative treatment, surface tension forces cause bordered pit membranes in heartwood and unseasoned sapwood to aspirate: the thickened central torus displaces against the pit aperture, forming an impermeable seal that prevents chemical flow between adjacent tracheids. Hardwoods present an entirely different anatomical challenge: fluid movement occurs predominantly through broad vessel elements rather than tracheids. However, in many dense hardwoods, vessels become occluded by cellular ingrowths termed tyloses, or are plugged by gummy deposits, rendering heartwood nearly impervious to preservative solutions.

Wood science and materials testing recognize substantial variations in treatability across commercial timber taxa. Highly receptive species, such as southern yellow pine (encompassing Pinus taeda, Pinus palustris, and Pinus echinata), possess wide sapwood bands whose bordered pits remain largely treatable under industrial pressure. Conversely, refractory timber taxa—notably coastal and interior Douglas-fir (Pseudotsuga menziesii), western hemlock (Tsuga heterophylla), white fir (Abies concolor), and white oak (Quercus alba)—resist chemical absorption even under sustained hydrostatic pressures. Microscopic verification of these anatomical characteristics is essential, as detailed in the technical guide to wood identification.

To overcome chemical refusal in refractory softwoods, industry standards mandate mechanical incising. Timber members are passed through heavy roller drums fitted with sharp, patterned incisor teeth that slit the wood grain to standard depths between 10 mm and 19 mm. Because longitudinal fluid penetration along exposed tracheid lumens proceeds twenty to fifty times faster than transverse radial or tangential penetration, incising exposes thousands of end-grain pathways across the timber surface. This mechanical conditioning ensures a continuous, uniform preservative shell that satisfies specified retention and penetration depths.

Industrial Treatment Processes: Pressure and Non-Pressure Systems

Industrial wood preservation methodologies are separated into pressure processes and non-pressure processes, differentiated by the hydrostatic forces employed to drive chemical biocide solutions into wood cellular cavities. Pressure treatments conducted inside hermetically sealed steel autoclaves represent the global standard for structural, exterior, and industrial wood applications, providing predictable chemical loading throughout the treatable sapwood boundary.

Pressure systems are engineered around two classical mechanical cycles: the full-cell process and the empty-cell process. The full-cell method (commonly known as the Bethell process) is engineered to maximize net chemical retention within both the cell walls and open cellular lumens. The treating cycle initiates with a deep initial vacuum (typically −75 kPa to −90 kPa gauge pressure for 30 to 60 minutes) to evacuate air from the timber pores. While sustaining the vacuum, the treating cylinder is flooded with preservative solution. Hydraulic pumps then pressurize the cylinder to 800 kPa to 1400 kPa (116 psi to 203 psi), forcing the liquid deep into the evacuated cellular matrix until refusal. A brief final vacuum removes excess surface dripping. The full-cell process is universally deployed for waterborne salts (such as copper-based formulations) and for heavy-duty marine pilings requiring maximum creosote loading.

Empty-cell processes are engineered to deeply coat internal cell walls while expelling excess liquid from cell lumens, minimizing gross chemical consumption and reducing member shipping weights. The Rueping process begins by applying initial air pressure (140 kPa to 400 kPa) into the cylinder, compressing air within the wood lumens prior to introducing the preservative. Once pressurized treating solution is driven into the wood and the hydraulic pressure is released, the trapped air expands vigorously, expelling surplus solution back into the working tank. The Lowry process achieves a comparable empty-cell effect without initial air pressure: the preservative is introduced at atmospheric pressure, hydraulic pressure is applied to achieve deep penetration, and a robust final vacuum recovers liquid held loosely in the cellular void spaces.

Non-pressure processes are utilized where autoclave infrastructure is unavailable, for temporary sapstain control, or for specialized field applications. In the thermal process (hot-and-cold bath), seasoned poles are submerged in hot preservative (80 °C to 105 °C) to heat and expand internal air, followed immediately by immersion in cold preservative (35 °C to 50 °C), creating a vacuum differential that draws chemical inward. Diffusion processes apply highly concentrated water-soluble borates or fluorides to green, unseasoned lumber; the chemical ions naturally migrate along internal moisture concentration gradients over several weeks of covered storage. Surface dip, spray, and brush applications provide thin chemical envelopes suitable for remedial field cuts or anti-sapstain protection during sawmill seasoning, but cannot provide structural ground contact protection. Furthermore, specialized thermal protocols are mandatory in export supply chains, as detailed in the operational framework for ISPM 15 wood packaging phytosanitary treatments requiring minimum 56 °C core heating for 30 continuous minutes.

AWPA Use Category System and Performance Standards

In North America, the selection, specification, and regulatory compliance of treated wood products are governed by the American Wood Protection Association (AWPA) Book of Standards, primarily AWPA Standard U1 (Use Category System: User Specification for Treated Wood). The Use Category System (UCS) provides a standardized, service-hazard hierarchy that aligns biological exposure risks with mandatory chemical retention and penetration thresholds across commercial wood species.

Standard U1 organizes service environments into five primary exposure categories, with subdivided hazard gradations:

  • UC1 (Interior, Dry): Wood installed in interior construction, fully shielded from exterior weather and free from moisture contact or condensation (for example, interior architectural millwork, furniture, and upper-floor structural joists).
  • UC2 (Interior, Damp): Protected interior wood that is subject to intermittent moisture, dampness, or condensation, such as mudsills, foundation plates over concrete slabs, and wet-room framing members.
  • UC3A (Exterior, Above Ground, Protected): Coated or painted exterior timbers configured for rapid water shed and continuous drying, including primed fascia, exterior window trim, and painted cladding.
  • UC3B (Exterior, Above Ground, Unprotected): Uncoated exterior timbers exposed to direct precipitation, prolonged wetting, and accumulation in joints, including residential deck boards, handrails, and horizontal fence rails.
  • UC4A (Ground Contact, General Use): Structural and landscape members installed in direct contact with soil or freshwater, including fence posts, deck substructure support posts, and garden landscape timbers.
  • UC4B (Ground Contact, Heavy Duty): Critical, difficult-to-replace structural elements exposed to severe soil decay hazards, including permanent wood foundation (PWF) framing, highway guardrail posts, utility distribution poles, and agricultural building posts.
  • UC4C (Ground Contact, Extreme Duty): High-hazard civil infrastructure components in severe decay zones, such as critical utility transmission poles and building foundation pilings in coastal environments.
  • UC5A, UC5B, and UC5C (Marine Saltwater Immersion): Structural pilings, bulkheads, and cross-bracing submerged in brackish or ocean waters, categorized by geographic marine borer aggressiveness (UC5A Northern waters; UC5B Central and Southern waters; UC5C Subtropical and Tropical waters with extreme Limnoria tripunctata and teredinid hazard).

As detailed in the data table below, chemical retention thresholds increase systematically as exposure hazard transitions from above-ground residential applications to ground-contact and marine environments. AWPA standards specify retention in weight of active biocide per unit volume of wood—expressed in pounds per cubic foot (pcf) or kilograms per cubic meter (kg/m³)—measured across an analytical assay zone extracted from standardized core borings.

Chemical Preservative Classes and EPA Regulatory Framework

Wood preservatives are classified chemically into waterborne, oil-borne, and organic solvent systems, each exhibiting distinct fixating kinetics, toxicological profiles, and environmental footprints. Under the Federal Insecticide, Fungicide, and Rodenticide Act (FIFRA), the US Environmental Protection Agency (EPA) regulates wood preservatives as antimicrobial pesticides, conducting mandatory 15-year cyclical registration reviews to assess occupational worker safety, consumer exposure, and ecological fate.

Modern residential lumber is dominated by waterborne copper formulations. Copper serves as a broad-spectrum fungicide that interferes with fungal cellular respiration by displacing essential metallic cofactors in fungal enzymes. However, because certain brown-rot fungi (notably Fibroporia radiculosa and Serpula lacrymans) display natural copper tolerance via oxalic acid production, copper formulations require secondary organic co-biocides:

  • Copper Azole (CA-B and CA-C): Combines soluble amine-copper with organic triazole fungicides (tebuconazole and propiconazole). CA-C is widely standardized for UC1 through UC4B applications, balancing broad antifungal coverage with reduced active ingredient loading.
  • Alkaline Copper Quaternary (ACQ-A through ACQ-D): Formulated with cupric oxide solubilized in ethanolamine or ammonium solutions, paired with a quaternary ammonium biocide (quaternary alkyl dimethyl benzyl ammonium chloride or didecyl dimethyl ammonium carbonate) that controls copper-tolerant fungi and insects.
  • Micronized Copper Systems (MCA and MCQ): Utilizes sub-micron, micro-milled basic copper carbonate particles (typically 1 nm to 250 nm) dispersed in water with specialized polymeric surfactants, rather than chemical amines. Micronized copper reduces active chemical leaching, yields a more natural lumber appearance, and substantially lessens galvanic corrosion rates on metal fasteners compared to soluble amine-copper formulations.
  • Inorganic Borates (SBX / Disodium Octaborate Tetrahydrate): Highly effective against subterranean termites and fungal decay, borates remain un-fixated salts. Because borate ions remain water-soluble, they leach rapidly if exposed to precipitation; consequently, borate treatments are strictly restricted to UC1 and UC2 interior framing and structural sill plates.

Heavy-duty civil and industrial sectors rely heavily on oil-borne and aromatic preservatives. Coal-tar creosote is a complex blend of aromatic hydrocarbons, polycyclic aromatic hydrocarbons (PAHs), and phenolic tar acids. Creosote provides exceptional moisture repellency and mechanical stabilization, making it the premier system for railroad crossties and marine bulkheads. Chromated Copper Arsenate (CCA-C)—which chemically fixates insoluble chromium, copper, and arsenic complexes within the wood cell walls—was voluntarily transitioned out of residential consumer lumber markets by manufacturers effective December 31, 2003, in agreement with the EPA. Today, CCA remains an EPA-registered restricted-use pesticide restricted strictly to industrial infrastructure, utility poles, agricultural poles, and marine pilings.

Regulatory oversight continues to reshape industrial chemical availability. In recent regulatory actions, the EPA issued cancellation decisions phasing out industrial pentachlorophenol (PCP) registrations due to health and environmental concerns. In response, utility pole treaters have transitioned to copper naphthenate (an organometallic complex in petroleum solvents) and 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one (DCOIT), an advanced organic biocide offering rapid environmental degradation without toxic metal bioaccumulation.

Standardized Laboratory and Field Testing Protocols

Before any novel chemical formulation or modified wood system is approved by consensus technical committees into AWPA Standard U1 or recognized in international building codes, it must undergo rigorous standardized testing. The AWPA Book of Standards and ASTM International define an exacting multi-phase testing framework ranging from bench-scale pure-culture bioassays to decades-long outdoor field stake evaluations.

The foundational laboratory screening protocol is the AWPA E10 Soil-Block Culture Assay (comparable to the historical ASTM D1413 standard). This method determines the threshold retention of a biocide: the minimum chemical loading required to suppress fungal decomposition below operational mass loss thresholds (typically defined as less than 2% to 3% net dry weight loss). The protocol proceeds through defined bench steps:

  1. Specimen Preparation: Uniform, straight-grained sapwood cubes measuring exactly 19.0 mm (0.75 in.) along each face are prepared from untreated southern pine (for testing against brown-rot fungi) or sweetgum/birch (for testing against white-rot fungi).
  2. Vacuum Impregnation: Replicate block cohorts are vacuum-impregnated with graded biocide dilutions, weighed to calculate gross chemical absorption, and conditioned under controlled atmospheric conditions.
  3. Weathering and Leaching Conditioning: Replicate test sets undergo water-leaching stress cycles (such as AWPA Standard E11, involving 14 days of agitated deionized water exchange) to simulate field weather exposure.
  4. Culture Jar Inoculation: Sterilized soil culture jars containing moist, loamy topsoil and feeder strips are inoculated with pure cultures of standard test fungi—such as Gloeophyllum trabeum (ATCC 11539), Fibroporia radiculosa (copper-tolerant brown rot), or Trametes versicolor (white rot).
  5. Incubation and Gravimetric Measurement: Test blocks are placed onto actively mycelium-covered feeder strips and incubated in darkness at 27 °C ± 1 °C and 70% ± 4% relative humidity for exactly 12 weeks. Following incubation, mycelium is carefully brushed off, the blocks are oven-dried at 103 °C, and percentage mass loss is calculated.

Formulations demonstrating efficacy in laboratory screening advance to outdoor empirical evaluations governed by the AWPA E7 Stake Test (analogous to ASTM D1758). Defect-free sapwood stakes (typically 19 × 19 × 457 mm or 50 × 100 × 457 mm) are pressure-treated with specified biocide retentions alongside untreated control stakes. These stakes are installed into outdoor field test plots located in regions with severe biological hazard ratings (such as Harrison County, Mississippi, or the tropical rainforest conditions of Hilo, Hawaii). Annually, stakes are extracted, physically probed, and assigned structural ratings: 10 (completely sound, no decay), 9 (trace superficial decay), 7 (moderate localized rot), 4 (heavy decay threatening integrity), and 0 (complete structural failure under light lateral breaking force). These long-term field stake arrays establish the definitive decay rates and service longevity benchmarks utilized in long-range forest inventory and timber cruise resource projections.

Operational Best Practices and Field Quality Assurance

Maximizing the operational performance of treated timber assemblies requires strict adherence to job-site handling protocols, fastener metallurgy standards, and field quality verification. Neglecting physical detailing or chemical integrity during field erection can compromise even high-retention structural components.

When pressure-treated lumber is cut, notched, or bored on-site, the fabrication process penetrates the outer treated protective shell and exposes unpenetrated heartwood or internal low-retention core zones to fungal spores and insect attack. AWPA Standard M4 mandates that all field cuts, cross-cuts, and drilled bolt holes must be liberally coated on-site with an approved remedial preservative. For members treated with copper-based waterborne systems or creosote, copper naphthenate solutions containing a minimum of 1.0% to 2.0% elemental copper are applied by repeated brushing or pressure-injection sleeves until saturation is achieved.

Fastener selection is another critical engineering consideration. Waterborne copper-treated wood contains elevated concentrations of soluble cupric ions that create an electrolytic cell when moisture bridges the wood and metal fasteners. Direct contact with standard electroplated zinc or mild carbon steel results in rapid galvanic fastener corrosion, leading to structural joint failure. Building codes mandate the use of hot-dip galvanized steel fasteners conforming to ASTM A153 (Class D coating) or high-grade stainless steel (AISI Type 304 or Type 316) for all connections in direct contact with copper-treated timbers, particularly in marine or coastal environments.

Quality assurance is verified by third-party inspection agencies accredited by the American Lumber Standard Committee (ALSC). Every commercial bundle or individual timber member carries an indelible plastic end-tag or ink stamp displaying the accredited inspection agency logo, the applicable AWPA Standard (such as AWPA U1), the specific Use Category designation (e.g., UC4A Ground Contact), the specific chemical preservative code, and the verified retention level. Field inspectors and procurement officers must verify these marks to ensure that above-ground grade lumber is never mistakenly buried in soil, a practice that represents the leading cause of premature structural failure in outdoor installations. Integrating durable, properly specified treated timber into long-term infrastructure supports the broader principles of sustainable forest management by maximizing structural replacement intervals.

Common Misunderstandings in Wood Preservation

A variety of technical misconceptions persist among end users, designers, and site contractors regarding the physical capabilities and limitations of preservative-treated forest products:

  • Myth 1: Pressure-treated lumber is waterproof. Chemical preservatives are biocide formulations designed exclusively to prevent fungal decay and insect consumption; they do not seal cellular lumens against moisture absorption. Treated wood readily absorbs ambient water, undergoes normal dimensional swelling and shrinkage across varying relative humidity, and will crack or check under solar heating unless coated with separate water-repellent sealers or penetrating stains.
  • Myth 2: Green surface discoloration indicates adequate preservative retention. The greenish hue characteristic of waterborne copper-treated wood results from basic copper salts reacting with timber extractives. Surface tinting does not reflect internal chemical retention or depth of penetration; furthermore, solar ultraviolet radiation photo-oxidizes surface copper within months, turning the wood silver-gray while internal chemical biocides remain fully active.
  • Myth 3: Any pressure-treated board can be installed in contact with the ground. Preservative-treated lumber is manufactured to specific retention tiers. Installing lumber stamped for UC3B (above-ground use) in direct ground contact guarantees premature biological rot within a few seasons, because soil contact harbors aggressive bacterial consortia and fungal loads that overwhelm lower above-ground chemical thresholds.
  • Myth 4: Borate-treated wood can be utilized outdoors if thoroughly painted. Inorganic borate salts (DOT / SBX) remain un-fixated within the wood matrix. Exterior temperature fluctuations and weathering inevitably create microscopic cracks and micro-fissures in paint coatings. Rainwater entering these fissures dissolves and rapidly leaches borate ions out of the wood, leaving the timber defenseless against decay fungi.
  • Myth 5: Burning scrap treated lumber in wood stoves or campfires is safe. Combustion of preservative-treated wood concentrates heavy metals and synthetic biocides in the fly ash and releases hazardous vapors. Burning treated wood is strictly prohibited by environmental regulations; all job-site scraps must be disposed of via designated municipal solid waste landfills.

Frequently asked questions

What is the difference between UC3B and UC4A treated wood?

AWPA Use Category UC3B designates wood intended exclusively for exterior, above-ground applications where members are exposed to direct precipitation but maintain rapid water runoff and do not contact soil, such as residential deck boards and railings. Use Category UC4A designates general-duty ground contact, engineered with substantially higher chemical retention thresholds (for example, 2.40 kg/m³ for Copper Azole CA-C, compared to 0.96 kg/m³ for UC3B) to resist continuous moisture and aggressive soil-borne decay fungi in fence posts and structural deck posts.

Why does heartwood resist chemical preservative penetration?

Heartwood resists fluid penetration because of extractive encrustation and anatomical pit aspiration. During heartwood formation in living trees, secondary metabolic compounds (polyphenols, resins, and gums) are deposited within cell walls and lumens. In softwoods, bordered pit membranes aspirate during drying—clamping shut against pit apertures—preventing lateral and longitudinal fluid transfer. Refractory heartwood species require mechanical incising to create artificial flow channels along the grain.

How does the AWPA E10 soil-block test determine threshold retention?

The AWPA E10 soil-block assay measures the decay resistance of 19 mm sapwood cubes treated with graded dilutions of preservative and exposed to pure cultures of wood-rotting basidiomycete fungi for 12 weeks at 27 °C and 70% relative humidity. Threshold retention is defined gravimetrically as the minimum biocide concentration that limits net dry mass loss of the wood block to less than 2% to 3%, identifying the minimum loading necessary to arrest fungal decomposition.

Can borate-treated wood be used in exterior structural applications?

No. Inorganic borates (Disodium Octaborate Tetrahydrate) do not chemically fixate or bond permanently to wood cell wall polymers. When exposed to outdoor precipitation, soil moisture, or standing water, water-soluble borate ions dissolve and leach out of the wood matrix, depleting biocide concentrations below insecticidal and fungicidal thresholds. Borate-treated lumber is restricted to UC1 and UC2 interior applications shielded from exterior liquid water.

Sources

  • USDA Forest Service, Forest Products Laboratory. Wood Handbook—Wood as an Engineering Material. General Technical Report FPL-GTR-282, Chapter 15: ‘Wood Preservatives’, by Grant T. Kirker and Stan T. Lebow. Madison, WI: U.S. Department of Agriculture, Forest Service, Forest Products Laboratory, 2021. https://research.fs.usda.gov/treesearch/62259 (accessed 2026-11-14).
  • US Environmental Protection Agency (EPA). ‘Overview of Wood Preservative Chemicals.’ Office of Pesticide Programs. https://www.epa.gov/ingredients-used-pesticide-products/overview-wood-preservative-chemicals (accessed 2026-11-14).
  • American Wood Protection Association (AWPA). AWPA Standard U1: Use Category System: User Specification for Treated Wood. Birmingham, AL: AWPA, 2023. https://awpa.com/standards/u1 (accessed 2026-11-14).
  • American Wood Protection Association (AWPA). AWPA Book of Standards: Evaluation Standards E7, E10, and E11. Birmingham, AL: AWPA, 2023. https://awpa.com (accessed 2026-11-14).

Data: Wood Preservative Specifications and AWPA Use Category Standards

Comparative technical specifications for major industrial and residential wood preservative systems, compiled from AWPA Standard U1 and USDA FPL-GTR-282, detailing chemical classifications, active ingredients, AWPA Use Categories, retention thresholds, and EPA regulatory status.

Period covered: 2021/2026. Coverage: United States.

Wood Preservative Specifications and AWPA Use Category Standards
Preservative SystemChemical ClassificationPrimary Active IngredientsAWPA Use CategoriesTarget Retention UC3B (kg/m³)Target Retention UC4A (kg/m³)Carrier SystemEPA Regulatory Status
Copper Azole Type C (CA-C)Waterborne organic-copper complexCopper, Tebuconazole, PropiconazoleUC1, UC2, UC3A, UC3B, UC4A, UC4B0.962.4Water (amine solvent)General use / residential and structural
Alkaline Copper Quat Type D (ACQ-D)Waterborne copper-amine complexCopper oxide (66.7%), Quaternary ammonium (33.3%)UC1, UC2, UC3A, UC3B, UC4A, UC4B2.46.4Water (ethanolamine solvent)General use / residential and structural
Micronized Copper Azole (MCA)Micro-milled particulate copper dispersionMicronized basic copper carbonate, TebuconazoleUC1, UC2, UC3A, UC3B, UC4A, UC4B0.962.4Water (surfactant dispersion)General use / residential and commercial
Inorganic Borate (SBX / DOT)Waterborne inorganic borate saltDisodium octaborate tetrahydrate (B2O3 equivalent)UC1, UC2 (interior and protected only)00Water (diffusion/pressure)General use / interior framing and millwork
Chromated Copper Arsenate Type C (CCA-C)Waterborne heavy metal saltChromium trioxide (47.5%), Copper oxide (18.5%), Arsenic pentoxide (34.0%)UC4A, UC4B, UC4C, UC5A, UC5B, UC5C46.4WaterRestricted use / industrial, marine, and utility only
Coal-Tar Creosote (CR)Oil-borne aromatic hydrocarbon distillatePolycyclic aromatic hydrocarbons (PAHs), Tar acids, Tar basesUC4A, UC4B, UC4C, UC5A, UC5B, UC5C128160Distillate oil / aromatic petroleumRestricted use / industrial crossties and pilings
Copper Naphthenate (CuN)Oil-borne organometallic compoundCopper salts of petroleum naphthenic acidsUC3B, UC4A, UC4B, UC4C0.641.28Heavy oil, light organic solvent, or water emulsionGeneral and restricted formulations / poles and remedial

Sources

Compiled by CASRAI from the sources above. Free to reuse under CC BY 4.0 with attribution.

Follow CASRAI

Research-administration guidance, standards updates and independent tool reviews.

Ask CASRAI · full access

Ask about Wood Preservation: Industrial Methods, Standards, and Testing Protocols

Full access: large monthly usage, up to 10 source passages behind each answer, and MCP and API access for Claude Code, Codex and other CLIs. Cancel any time.

An AI assistant for research: funder rules, compliance, methods and publishing. It links the sources behind its answers and labels answers that come from a web search.

Answers draw on CASRAI's guides and dictionary plus the federal and funder documents we index: Federal Register, Grants.gov, Regulations.gov and UKRI.

Works on this site and inside Claude, Cursor and the AI tools you already use.

Everything CASRAI publishes — this page, the dictionary, the guides and the news — stays open to read, with no account and no card.

Referenced across the research world

University of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logoUniversity of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logo
  • University of Cambridge logo
  • Columbia University logo
  • Crossref logo
  • University of Edinburgh logo
  • Harvard University logo
  • University of Oxford logo
  • Princeton University logo
  • Stanford School of Medicine logo
  • University College London logo
  • ORCID logo

View CASRAI adoption →