Skip to main content
v2026.11,986 entries · CC-BY 4.0

Hot Isostatic Pressing (HIP): Parameters and Limits

How hot isostatic pressing closes internal pores, the pressure and temperature ranges reported, what it cannot fix, and which ASTM documents apply.

Written and maintained by CASRAI Editorial Board

Published

On this page

Hot isostatic pressing (HIP) is a process that applies high temperature and high gas pressure to a part at the same time, so that internal voids in a casting, sintered compact or additively manufactured metal part close and the material becomes denser. The pressure is isostatic, meaning equal in all directions, and is usually supplied by an inert gas such as argon. HIP closes internal pores; it does not close pores that are connected to the surface.

Short answer

HIP puts a component inside a heated pressure vessel, raises temperature and gas pressure together, holds them, then cools and releases the gas. According to the Open University’s OpenLearn material on the process, typical pressures are 50 to 200 MPa and temperatures reach up to 2000 °C depending on the material, with hold times of roughly 1 to 4 hours and complete cycles of about 2 to 6 hours. Its main use is to remove internal porosity that would otherwise act as a starting point for fatigue cracks.

Definition and scope

OpenLearn describes HIP as the simultaneous application of high temperature and pressure to cast or sintered parts, with argon gas in the furnace providing the isostatic pressure, which fills pores and improves density. ASTM A1080/A1080M describes the same idea for castings: heat and pressure are applied simultaneously in an autoclave using an inert gas, with the purpose of eliminating internal voids and obtaining the desired properties.

Three variables define a HIP cycle: temperature, pressure and duration. NASA’s technical memorandum on HIP of additively manufactured Inconel 718 (NASA/TM-20210015451, May 2021) names exactly these as the HIP parameters and states that pore closure depends on pore shape, trapped gas and those parameters.

The process sits in the powder-metallurgy and materials-processing family. Our guide to powder metallurgy covers the broader routes by which powder becomes a solid component; HIP is one of the ways to reach near-full density. It is also one of several thermal post-processing steps applied to metal parts built by powder bed fusion, which is where much current laboratory and research interest in HIP comes from.

This page is a general explainer for researchers, laboratory staff and anyone specifying or reading a materials-processing report. It does not provide a cycle recipe for any alloy; cycle parameters are material-specific and belong in the governing specification or the process supplier’s qualified procedure.

How HIP works in practice

OpenLearn outlines the sequence in three stages. First, the part is loaded into the furnace, which sits inside the pressure vessel. Second, pressure and temperature are raised simultaneously and held. Third, the vessel is cooled and the gas is released, and OpenLearn notes the gas can be recycled.

What the parameters look like

Temperature depends on the material. OpenLearn gives two worked examples: about 900 °C for the titanium alloy Ti-6Al-4V and about 500 °C for the aluminium casting alloy Al-7.5Si-0.5Mg. It states that temperature in the equipment is controllable to within about ±15 °C. The pressure range it quotes is 50 to 200 MPa, and it cites hold times of around 1 to 4 hours within a total cycle of about 2 to 6 hours.

These are illustrative values from one educational source, which itself is more than eight years old, so equipment size limits and cost statements in it should be treated as indicative rather than current. For comparison, the NASA memorandum uses a baseline simulated hold of 1163 °C and 103 MPa for Inconel 718. That figure is a modelling baseline supplied by the project, not a standard cycle, and the model’s results were not completed against CT validation, so it should be read as a simulation input only. The practical lesson is that no single temperature, pressure or time applies across alloys.

What happens to the pores

Under temperature and pressure the surrounding material deforms and the internal pore collapses, and the faces of the pore can fuse. NASA describes this for selective laser melted (SLM) Inconel 718, where HIP is applied after the build to reduce porosity because pores act as stress risers and crack-initiation sites that reduce fatigue life.

Direct measurement supports the effect. Tammas-Williams, Withers, Todd and Prangnell (2016, Metallurgical and Materials Transactions A 47(5):1939-1946) used X-ray computed tomography before and after a standard HIP cycle on worst-case Ti-6Al-4V samples made by selective electron beam melting. They report that all internal porosity was shrunk to below the resolution limit of the CT measurement, apart from defects that had surface-connected ligaments. For how that imaging method works and what it can and cannot resolve, see our guide to micro-CT.

What HIP closes and what it does not

The distinction that matters most when reading a HIP claim is between internal pores and pores that reach the surface. The table below combines what the three technical sources state.

Defect or condition Effect of HIP according to the sources Source
Fully enclosed (internal) pores Close and fuse under heat and pressure; in the Ti-6Al-4V electron beam study they shrank below the CT resolution limit OpenLearn; NASA/TM-20210015451; Tammas-Williams et al. 2016
Pores connected to the surface Not closed; OpenLearn says HIP closes internal but not surface-connected porosity, and Tammas-Williams et al. found defects with surface-connected ligaments remained OpenLearn; Tammas-Williams et al. 2016
Pores containing trapped gas Closure depends on trapped gas; NASA attributes residual porosity after HIP partly to trapped argon, citing prior work NASA/TM-20210015451
Strength after HIP OpenLearn reports only a slight tensile gain; the larger gains are in creep and fatigue behaviour (it cites fatigue life improvements of roughly 1.5 to 8 times) OpenLearn
Microstructure after HIP NASA notes that additional heat treatments are needed to recover the optimal properties after HIP NASA/TM-20210015451

Treat any claim that HIP removes all porosity with caution: the sources consistently limit the effect to internal pores and tie residual porosity to surface connection and trapped gas.

HIP and sintering

Sintering consolidates powder with heat. OpenLearn lists sintered parts alongside castings as HIP candidates, which means HIP can follow sintering to close the remaining internal porosity. Our guide on powder metallurgy notes that reaching full density requires routes such as HIP.

HIP of castings

For castings, OpenLearn lists uses including improving tensile, creep and fatigue behaviour, homogenising the casting and salvaging porous castings. It also describes HIP being used to rejuvenate creep-damaged turbine blades. Typical sectors it names include aerospace, pump impellers and prostheses.

HIP as additive manufacturing post-processing

Both the NASA memorandum and the Ti-6Al-4V study address HIP of additively manufactured metal, where lack-of-fusion voids and gas pores left by the build are the targets. HIP is therefore a post-processing step with its own parameters, not a build parameter. Our guide to metal powder for 3D printing covers the feedstock end of the same workflow, and metal injection moulding is another powder route in which densification is a central concern.

Where it matters for labs, qualification and standards

Because HIP changes internal quality but not surface condition, the way a laboratory verifies the result matters as much as the cycle. The sources point to three practical checks. The first is internal porosity measurement, as in the CT approach above. The second is mechanical behaviour, particularly fatigue and creep, where OpenLearn locates the largest benefit. The third is confirming that any additional heat treatment required after HIP, as NASA notes, has been specified. For tensile data on HIP-treated material, see our guide to the tensile test.

Standards that mention HIP are narrower than the process. The data table below lists three ASTM documents, their scope as stated on the ASTM store pages (read 2026-11-13), and whether HIP is named on the page. In summary:

  • ASTM A1080/A1080M-24 is a standard practice for HIP of steel, stainless steel and related alloy castings. It covers general requirements including quality requirements, autoclave type and qualification, temperature uniformity, temperature and pressure measurement and control, and gas measurement.
  • ASTM A988/A988M-26 is a specification for hot isostatically pressed powder-metallurgy stainless steel piping components for pressure systems, with A989/A989M as the parallel document for alloy steel.
  • ASTM F3301-18a is a specification for thermal post-processing of metal parts made by powder bed fusion and lists materials such as Ti-6Al-4V, UNS N07718 and AlSi10Mg. The store page does not mention HIP, so it should not be cited as a HIP specification without reading the full standard.

The standard-citation convention for these documents, including edition designators, is covered in our guide on how to cite ASTM standards. When citing one, state the designation with its year suffix, as the active edition changes.

Common misunderstandings

HIP repairs surface cracks

It does not. Per OpenLearn and the electron beam study, surface-connected porosity remains after HIP. Surface-breaking defects require other treatments or rejection.

HIP restores full properties

Closing pores improves fatigue and creep behaviour, but NASA notes additional heat treatments are needed to recover optimal properties after HIP, and OpenLearn reports only a slight tensile gain.

One cycle suits all materials

OpenLearn’s own examples differ by around 400 °C between a titanium alloy and an aluminium casting alloy. The NASA baseline differs again. Cycle parameters belong to the alloy and the governing specification.

The simulated baseline is a standard cycle

The NASA figures are the model’s baseline, supplied by the project, and the report’s simulation was not completed against CT validation.

FAQ

What is hot isostatic pressing?

A process that applies high temperature and high isostatic gas pressure together to a component to close internal pores and increase density. OpenLearn and ASTM A1080/A1080M both describe it in these terms.

What pressure and temperature does HIP use?

OpenLearn gives 50 to 200 MPa and temperatures up to 2000 °C depending on material, with examples of about 900 °C for Ti-6Al-4V and about 500 °C for Al-7.5Si-0.5Mg. Values for a specific alloy come from its specification or supplier procedure.

How long does a HIP cycle take?

OpenLearn cites hold times of roughly 1 to 4 hours and complete cycles of about 2 to 6 hours.

Does HIP close surface pores?

No. HIP closes internal porosity; defects with surface-connected ligaments remained in the Ti-6Al-4V CT study, and OpenLearn says surface-connected porosity is not closed.

Why is HIP used on 3D-printed metal parts?

Because pores in additively manufactured metal act as stress risers and crack-initiation sites that reduce fatigue life, as NASA states for SLM Inconel 718.

Which standard covers HIP?

For castings, ASTM A1080/A1080M-24 is a standard practice for HIP of steel, stainless steel and related alloy castings. For powder-metallurgy piping components, see ASTM A988/A988M and A989/A989M.

Sources

  • The Open University, OpenLearn, “Hot isostatic pressing (HIP)”: open.edu/openlearn. Read 2026-11-13.
  • Fody and Lang, “Hot Isostatic Pressing for Reduction of Defects in Additively Manufactured Inconel-718”, NASA/TM-20210015451, May 2021: NASA Technical Reports Server. Read 2026-11-13.
  • Tammas-Williams, Withers, Todd and Prangnell (2016), “The Effectiveness of Hot Isostatic Pressing for Closing Porosity in Titanium Parts Manufactured by Selective Electron Beam Melting”, Metallurgical and Materials Transactions A 47(5):1939-1946: White Rose Research Online. Read 2026-11-13.
  • ASTM A1080/A1080M-24: ASTM store page. Read 2026-11-13.
  • ASTM A988/A988M-26: ASTM store page. Read 2026-11-13.
  • ASTM F3301-18a: ASTM store page. Read 2026-11-13.

Data: ASTM documents relevant to hot isostatic pressing and powder-metal post-processing

Compares three ASTM documents by title, material scope, product form and whether the ASTM store page names hot isostatic pressing, compiled from the ASTM store pages read on 2026-11-13.

Period covered: 2018/2026.

ASTM documents relevant to hot isostatic pressing and powder-metal post-processing
ASTM documentDocument typeMaterial or product scopeHot isostatic pressing named on store page
ASTM A1080/A1080M-24Standard practiceSteel, stainless steel and related alloy castingsYes (practice for HIP of castings; covers autoclave qualification, temperature uniformity, temperature and pressure measurement and control)
ASTM A988/A988M-26SpecificationHot isostatically pressed powder-metallurgy stainless steel piping components for pressure systemsYes (product is HIP powder-metallurgy)
ASTM F3301-18aSpecificationThermal post-processing of metal parts made by powder bed fusion (Ti-6Al-4V, CP Ti, Co-28Cr-6Mo, UNS N07718, N06625, S31603, AlSi10Mg)No

Sources

Compiled by CASRAI from the sources above. Free to reuse under CC BY 4.0 with attribution.

Follow CASRAI

Research-administration guidance, standards updates and independent tool reviews.

Ask CASRAI · full access

Ask about Hot Isostatic Pressing (HIP): Parameters and Limits

Full access: large monthly usage, up to 10 source passages behind each answer, and MCP and API access for Claude Code, Codex and other CLIs. Cancel any time.

An AI assistant for research: funder rules, compliance, methods and publishing. It links the sources behind its answers and labels answers that come from a web search.

Answers draw on CASRAI's guides and dictionary plus the federal and funder documents we index: Federal Register, Grants.gov, Regulations.gov and UKRI.

Works on this site and inside Claude, Cursor and the AI tools you already use.

Everything CASRAI publishes — this page, the dictionary, the guides and the news — stays open to read, with no account and no card.

Referenced across the research world

University of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logoUniversity of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logo
  • University of Cambridge logo
  • Columbia University logo
  • Crossref logo
  • University of Edinburgh logo
  • Harvard University logo
  • University of Oxford logo
  • Princeton University logo
  • Stanford School of Medicine logo
  • University College London logo
  • ORCID logo

View CASRAI adoption →