How hybrid bonding joins Cu pads and dielectric without solder: process flow, SiO2 vs SiCN, and imec’s reported wafer and die-to-wafer pitch results.

Written and maintained by CASRAI Editorial Board

Published

On this page

Hybrid bonding is a way of joining two semiconductor components face to face so that copper pads bond directly to copper pads and the surrounding dielectric bonds directly to dielectric, with no solder bump or adhesive layer between them. The surfaces are planarised by chemical mechanical polishing (CMP), pressed together at room temperature and then annealed so the dielectric and copper bonds become permanent. imec, the Belgian research centre whose published results this guide relies on, has reported it at 400 nm interconnect pitch on 300 mm wafers and at 2 µm pitch for dies placed on wafers.

What is hybrid bonding?

imec describes wafer-to-wafer hybrid bonding as Cu-to-Cu and dielectric-to-dielectric 3D integration, in which copper damascene structures define the bonding surfaces. The word “hybrid” refers to the two materials that bond at the same time on one interface: copper pads that carry the electrical signals, and the dielectric around them that holds the two sides together. Adeia, a company that licenses a hybrid bonding technology under the name direct bond interconnect (DBI), describes hybrid bonding in a June 2024 release as an advanced semiconductor packaging technology that integrates different functional elements such as logic, memory and sensors, and that improves electrical and thermal performance.

The reason the technique matters is pitch, the centre-to-centre spacing of the interconnects. imec states that the state of the art in commercial wafer-to-wafer hybrid bonding is a copper interconnect pitch of about 1 µm, which corresponds to about a million interconnects per square millimetre, and that stacking memory on logic needs a pitch far below 1 µm. The same imec research update names stacked image sensors and the CMOS peripheral circuitry of 3D NAND as commercial applications of wafer-to-wafer hybrid bonding.

How the process flow works

The wafer-to-wafer flow that imec publishes begins with two fully processed 300 mm wafers, meaning the front-end-of-line and back-end-of-line work is finished. The steps that follow are the same ones that appear in every discussion of the technique, and each of them is where a particular risk sits.

  1. Etch cavities in the bonding dielectric. The dielectric is mainly SiO2 in today’s flows.
  2. Fill the cavities with a barrier metal, a seed layer and copper. This is the damascene step, and it defines the copper pads that will later meet their counterparts on the other wafer.
  3. Planarise with CMP. imec says the CMP is optimised for high uniformity across the wafer and leaves a flat dielectric surface with the copper pads recessed by a few nanometres.
  4. Align the wafers accurately. The alignment, reported as overlay, decides whether each copper pad lands on its partner.
  5. Bond at room temperature. Bonding starts at the centre of the wafer, and a bonding wave closes the gap towards the edge.
  6. Anneal at a higher temperature. The anneal turns the room-temperature contact into the permanent dielectric-to-dielectric and copper-to-copper bonds.

The recess in step 3 is deliberate. imec explains that the copper has to sit a few nanometres below the dielectric surface so that, after the anneal, the bond is free of voids. The same research update adds that advanced CMP combined with dummy pads in the layout is used to control surface topography. imec names three challenges for the technique at small pitch: copper-to-copper alignment accuracy, wafer purity and topology before bonding, and the bond strength of dielectrics and copper pads.

SiO2 or SiCN: the dielectric choice

imec reports that SiO2 is the predominant bonding dielectric, and that SiCN has been proposed for small pitches. According to imec, SiCN has a higher bonding energy than SiO2, acts as a copper diffusion barrier and as a wafer passivation layer that blocks gas diffusion, and is thermally stable. Nanoindentation measurements cited by imec showed that the SiCN-to-SiCN bond strength significantly outperforms the SiO2-to-SiO2 bond strength. The high bond strength is reached after a post-bond anneal at 250 °C and does not degrade at higher temperatures. Both of imec’s reported results in the data table below use a Cu/SiCN combination.

Wafer-to-wafer and die-to-wafer hybrid bonding

The two variants that imec reports differ in what is bonded to what.

Wafer-to-wafer (W2W)

Whole wafers are bonded, so every die position on one wafer is joined to the matching position on the other. At the IEDM 2023 conference imec presented 400 nm interconnect pitch on 300 mm wafers, bonded with a commercial high-quality wafer bonder with advanced alignment, with a wafer-to-wafer overlay below 150 nm, low single-contact resistance and good control of the Cu/SiCN surface topography. imec states that at 400 nm pitch the overlay has to be below 100 nm to give enough yield in high-volume manufacturing, so the reported 150 nm is an intermediate result and not a production figure. imec also reports a pad layout that is new in this work: a hexagonal grid of circular copper pads, which gives the densest packing with equal distance to every neighbour, in place of the traditional square grid. An unequal pad design, in which the top wafer has smaller critical copper pad dimensions than the bottom one, gave greater overlay tolerance, lower parasitic capacitance and higher dielectric breakdown strength at small pitch.

Die-to-wafer (D2W)

Individual dies are placed on a wafer. imec reported at IEEE ECTC 2024 (coverage dated 29 May 2024) the first demonstration of Cu-to-Cu and SiCN-to-SiCN die-to-wafer bonding at a 2 µm copper bond pad pitch, with a die-to-wafer overlay error below 350 nm that it attributes to the die processing and a high-accuracy pick-and-place step. The copper recess was kept below 2.5 nm through tight CMP optimisation of the Cu/SiCN surface, and the dies were separated by plasma dicing to avoid particles and damage to that surface. At 2 µm pitch imec reported a Kelvin electrical yield above 85% and a daisy-chain electrical yield above 70%. imec’s stated aim is to push the pitch towards 1 µm. The same work coupled photonic IC dies to a 300 mm bottom optical interconnect wafer through collective SiCN-based die-to-wafer assembly, with coupling losses below 0.5 dB, which links the technique to the photonic integrated circuit field.

The data table below puts these reported results side by side, together with the solder-based comparison point that imec cites. All values are imec’s own reports and are laboratory demonstrations, not statements about what any factory ships.

How hybrid bonding differs from solder bumps and adhesives

A solder-bump interconnect, as used in flip-chip assembly, joins two parts through discrete bumps of solder. Hybrid bonding has no bump: the copper pads sit a few nanometres below a planarised dielectric surface and the two surfaces meet directly. imec’s own comparison, in the 2024 die-to-wafer report, is that solder-based die-to-wafer bonding is likely to stagnate at a bump pitch of 10 to 5 µm, while wafer-to-wafer hybrid bonding has already reached 400 nm and may reach 200 nm in the future. The reported pitch gap, roughly an order of magnitude in imec’s numbers, is the main reason the technique is studied for dense 3D stacking and for the broader field of wafer-level packaging.

It also differs from adhesive bonding. In imec’s description of hybrid bonding the permanent bond is formed by the dielectric surfaces and the copper pads themselves after the anneal, with no separate adhesive layer in the flow, and Adeia likewise calls its approach direct bond interconnect.

Where it matters for fabs, labs and supply decisions

For anyone who specifies, operates or qualifies equipment around this process, the imec figures point to where the tight requirements sit. They are reported process capabilities, not procurement criteria.

  • Alignment and overlay. The overlay budget shrinks with the pitch: below 150 nm was reported at 400 nm pitch for wafers, and below 350 nm at 2 µm pitch for dies. imec says the wafer result relied on a commercial wafer bonder with advanced alignment.
  • Surface topography. Recesses are specified in nanometres (a few nanometres for wafers, below 2.5 nm for the die-to-wafer work), so the CMP step and its across-wafer uniformity are central.
  • Particles and surface cleanliness. imec lists wafer purity and topology as challenges and chose plasma dicing for dies so that particles and damage do not reach the bonding surface.
  • Post-bond processing. In a backside power delivery network flow, part of the back-end-of-line processing, the power delivery lines, takes place after bonding: the front side of the first wafer is bonded to a carrier, the backside is thinned, and n-TSV patterning, metal fill and backside metallisation follow.
  • Licensing. Adeia states that Kioxia and Western Digital entered a long-term agreement in 2023 to license its semiconductor patent portfolio, including hybrid bonding patents, so some implementations of the process are covered by licensed patents.

Common misunderstandings

  • “Hybrid” does not mean a mix of solder and adhesive. It refers to the two materials, copper and dielectric, that bond on the same interface.
  • The anneal is not what makes first contact. imec’s flow bonds at room temperature and uses the higher-temperature anneal afterwards to make the bonds permanent. For SiCN, imec reports the strong bond after a 250 °C post-bond anneal.
  • A published pitch is not a production pitch. The 400 nm and 2 µm figures are research demonstrations. imec itself contrasts the 400 nm result with the roughly 1 µm of today’s commercial applications.
  • Overlay results are not yield results. imec states the overlay target needed for high-volume yield at 400 nm pitch (below 100 nm) separately from the 150 nm it achieved.
  • Die-to-wafer and wafer-to-wafer figures are not interchangeable. The die-to-wafer work is at 2 µm pitch with overlay below 350 nm and reported electrical yields, while the wafer-to-wafer work is at 400 nm with overlay below 150 nm; they are different experiments and should not be read as one scale.

Sources

Data: Reported hybrid bonding results from imec and the solder comparison point

Compiled from imec's published wafer-to-wafer (IEDM 2023) and die-to-wafer (IEEE ECTC 2024) hybrid bonding results, plus the commercial pitch and solder-bump comparison points imec cites. All values are as reported by imec and are laboratory demonstrations or imec statements, not production specifications.

Period covered: 2023/2024.

Reported hybrid bonding results from imec and the solder comparison point
CaseReported pitch (µm)Overlay (nm)Cu pad recess (nm)Electrical yieldVenue and note
W2W Cu/SiCN on 300 mm wafers0.4below 150a fewnot reportedIEDM 2023; imec states overlay below 100 nm is needed for high-volume yield at this pitch
D2W Cu/SiCN dies on a wafer2below 350below 2.5Kelvin above 85%; daisy chain above 70%IEEE ECTC 2024; plasma dicing; imec aims for 1 µm pitch
W2W in today's commercial applications (imec)1not reportednot reportednot reportedimec: about 1 µm, about a million interconnects per mm2
Solder-based D2W (imec outlook)5 to 10not reportednot applicablenot reportedimec: likely to stagnate at 10 to 5 µm bump pitch

Sources

Compiled by CASRAI from the sources above. Free to reuse under CC BY 4.0 with attribution.

Follow CASRAI

Research-administration guidance, standards updates and independent tool reviews.

Ask CASRAI · full access

Ask about Hybrid Bonding: Process, Dielectrics and Reported Pitch Results

Full access: large monthly usage, up to 10 source passages behind each answer, and MCP and API access for Claude Code, Codex and other CLIs. Cancel any time.

An AI assistant for research: funder rules, compliance, methods and publishing. It links the sources behind its answers and labels answers that come from a web search.

Answers draw on CASRAI's guides and dictionary plus the federal and funder documents we index: Federal Register, Grants.gov, Regulations.gov and UKRI.

Works on this site and inside Claude, Cursor and the AI tools you already use.

Everything CASRAI publishes — this page, the dictionary, the guides and the news — stays open to read, with no account and no card.

Referenced across the research world

University of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logoUniversity of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logo
  • University of Cambridge logo
  • Columbia University logo
  • Crossref logo
  • University of Edinburgh logo
  • Harvard University logo
  • University of Oxford logo
  • Princeton University logo
  • Stanford School of Medicine logo
  • University College London logo
  • ORCID logo

View CASRAI adoption →