Written and maintained by CASRAI Editorial Board
Published
On this page
The Larson-Miller parameter (LMP) is a time-temperature parameter used to correlate creep-rupture data: it combines absolute temperature T and rupture time t_r into one number, P = T(C + log t_r), where C is a material constant usually taken as about 20 when t_r is in hours. Tests run hot and short are then used to estimate rupture life at lower temperatures and longer times.
Short answer
Use the LMP when you have creep-rupture or stress-rupture data at several temperatures and need to estimate how long a metal survives at a service temperature that was not tested. At a fixed applied stress, test points that differ in temperature and time collapse onto one value of P, so a short, hot test stands in for a long, cooler one. The estimate depends heavily on the constant C and on how far you extrapolate, which is why both belong in every report.
Definition and scope
The parameter is written P = T(C + log t_r). T is absolute temperature (kelvin or degrees Rankine), t_r is time to rupture, log is the base-10 logarithm and C is an empirical constant. The relation was published by Larson and Miller in a 1952 paper in the Transactions of the ASME (volume 74), and it is still one of the classical extrapolation methods alongside Orr-Sherby-Dorn, Manson-Haferd and Wilshire, as listed in a 2025 paper on long-term serviced Grade 91 steel in Frontiers in Materials.
Rearranged, the same relation is a straight line: log t_r = P/T – C. At one applied stress, plotting log t_r against 1/T gives a line whose slope is P (a function of stress) and whose intercept is -C. The Frontiers paper uses this iso-stress form, with T in kelvin and t_r in hours, and notes that it presumes the relationship between log t_r and 1/T is linear.
Scope matters. The LMP correlates time and temperature for rupture (and, in the same way, for other quantities such as applied stress). It is not a test method and not a material specification. Inspectioneering describes it as an extrapolation technique for correlating time and temperature, used to estimate time to stress rupture against operating metal temperature. The data that feed it come from creep and stress-rupture testing, covered by ASTM E139-24, which addresses creep (deformation versus time at constant tensile force and temperature) and rupture (time to failure) tests of metallic materials, including equipment and reporting requirements.
How the LMP is used in practice
From test data to an estimate
The workflow below is the iso-stress method described in the Frontiers paper, which typically needs data at three or more temperatures about 25 degrees C apart.
- Run creep-rupture tests at one applied stress and several temperatures, recording rupture time in hours.
- Convert temperatures to kelvin and plot log t_r against 1/T. A straight line is the assumption behind the LMP.
- Read the slope (P at that stress) and the intercept (-C). Repeat for other stress levels.
- Choose the service temperature of interest and solve log t_r = P/T – C for t_r.
Practitioners often skip the fit of C and use a conventional value, then look up P for a given stress from tabulated data. Inspectioneering notes that API 530 gives creep-rupture data (minimum and average properties) in terms of the LMP, and that this is commonly used for fired-heater tube thickness and remaining-life estimates.
Worked arithmetic (illustrative, not material data)
The numbers below are a self-computed illustration of the formula, using C = 20, t in hours and T in kelvin. They describe no real alloy.
A test ruptures after 10,000 h at 923 K. Since log 10,000 = 4, P = 923 x (20 + 4) = 923 x 24 = 22,152. If the same P applies at 973 K, then C + log t = 22,152 / 973 = 22.767, so log t = 2.767 and t is about 584 h. Hotter by 50 K, rupture comes roughly 17 times sooner under these assumptions.
The unit convention changes the number. P computed with T in degrees Rankine is 1.8 times the value computed with T in kelvin, so a table of P values is only usable if its temperature scale and its constant C are stated.
Types and related concepts: the constant C and its sensitivity
C is the weak point of the method. In the Frontiers study of Grade 91 steel, fitted values of C ranged from 18 to 21 for base metal and from 16 to 21 for welded joints, while the standard values were about 21 (base metal) and about 23 (welded joints) at low stress. The data table below compares these sourced values.
The same paper states that a larger C gives a longer evaluated life at low temperature, and that shifting C by plus or minus 3 changed the estimate at 600 degrees C by a factor of roughly 0.75 to 1.45 when extrapolating from 650 degrees C and 10,000 h. The following table is an illustration of that mechanism, computed here with the formula above for a single point at 650 degrees C (923.15 K) and 10,000 h extrapolated to 600 degrees C (873.15 K). It is arithmetic, not data for any material, and it uses a single-point extrapolation, so it differs from the paper’s fitted result.
| Assumed C | P = T(C + log t_r), K | Estimated t_r at 873.15 K, hours | Relative to C = 20 |
|---|---|---|---|
| 17 | 19,386 | about 159,000 | 0.67 |
| 18 | 20,309 | about 182,000 | 0.77 |
| 20 | 22,156 | about 237,000 | 1.00 |
| 21 | 23,079 | about 270,000 | 1.14 |
| 23 | 24,925 | about 352,000 | 1.49 |
One practical point follows: a constant chosen by convention can move a life estimate by tens of percent, and the effect grows with the temperature gap between tests and service.
Why C is about 20
A value near 20 is a convention. A 2018 paper by Maruyama and co-workers in the International Journal of Pressure Vessels and Piping, “On the physical basis of a Larson-Miller constant of 20” (volume 159, pages 93-100), examines whether that value has a physical basis. It is a reminder to treat C as an empirical fitting constant unless the dataset supports a specific value.
Related approaches
The Frontiers paper lists Orr-Sherby-Dorn, Manson-Haferd and Wilshire as other classical extrapolation methods. Inspectioneering describes the MPC Omega method in API 579-1/ASME FFS-1 Part 10 as a strain-rate-based alternative to the LMP for remaining-life assessment. The LMP is the simplest of these because it has a single adjustable constant, which is also why it is the most sensitive to that choice.
Where it matters for labs and materials testing
For a materials laboratory, the LMP decides what to test and what can be claimed. Long creep tests run for years, so a plan usually uses shorter tests at higher temperatures and then extrapolates. Three sourced cautions shape that plan:
- Extrapolation range. The Frontiers paper notes that the reliability of these extrapolations is often questioned beyond 100,000 h for Grade 91 and 92 steels. Report the extrapolation factor (target life divided by longest test) next to any estimate.
- Linearity. The linear 1/T assumption may not apply to virgin Grade 91 steels, where the behaviour is nonlinear, so the fit has to be checked on your own data rather than assumed.
- Small changes in service conditions. Inspectioneering stresses that small changes in long-term metal temperature or stress strongly change remaining life, and that excursions should be included in an assessment.
Test records also need to be traceable. ASTM E139-24 is the standard for conducting the underlying creep, creep-rupture and stress-rupture tests, and it excludes notched specimens (covered by Practice E292) and short-time tests (Test Methods E21). If you publish LMP results, cite the standard edition used; see our guide on how to cite ASTM standards and the ASTM Compass overview. For the related short-time test, see the tensile test guide, and for the field in general what materials science is. Where creep datasets are shared openly, the Materials Genome Initiative and FAIR materials data guide describes the data-sharing context.
Reporting checklist
This checklist is an editorial synthesis of the sourced cautions above, not a published standard. A reader should be able to reproduce any LMP value from the following items.
- Units: temperature scale (K or Rankine), time unit (hours) and logarithm base (10).
- Source of C: fitted from the reported data (with the fit range), or a conventional value.
- Applied stress for each iso-stress line and the number of test temperatures.
- Longest test duration and the target life, so the extrapolation factor is visible.
- Material and condition (base metal or welded joint), since the Grade 91 figures differ between them.
- The test standard and edition used to generate the data.
Common misunderstandings
- C is a universal constant. It is empirical. The Grade 91 figures above range from 16 to 23 depending on condition and on whether it was fitted or taken as a standard value.
- The same P means the same life for any material. P correlates time and temperature within a material and stress, not across materials.
- More digits mean more certainty. A life estimate computed to four figures inherits the uncertainty of C and of the extrapolation.
- The LMP replaces testing. It extrapolates from tests, and the tests themselves follow standards such as ASTM E139.
- It is the only method. Other correlation methods and the API 579-1 Omega method exist, and the Omega method is strain-rate based.
Sources
- Frontiers in Materials: Temperature dependence of creep rupture life of long-term serviced Grade 91 steel (Yaguchi, Kanai, Tamura, 2025), checked 2026-11-18
- Inspectioneering: Damage Control: High-Temperature Creep Assessment, checked 2026-11-18
- ASTM International: E0139-24, Standard Test Methods for Conducting Creep, Creep-Rupture, and Stress-Rupture Tests of Metallic Materials, checked 2026-11-18
- NIMS SAMURAI: On the physical basis of a Larson-Miller constant of 20 (Maruyama et al., 2018), checked 2026-11-18
- Wikipedia: Larson-Miller relation, checked 2026-11-18
Data: Larson-Miller constant C values reported for Grade 91 steel
Values of the Larson-Miller constant C for Grade 91 steel base metal and welded joints, compiled from a 2025 Frontiers in Materials paper on long-term serviced Grade 91 steel. Fitted ranges and standard values are listed separately; C is dimensionless with time in hours and temperature in kelvin.
| Material condition and basis | C, lower value | C, upper value |
|---|---|---|
| Base metal, fitted to creep-rupture data | 18 | 21 |
| Welded joints, fitted to creep-rupture data | 16 | 21 |
| Base metal, standard value at low stress (about) | 21 | 21 |
| Welded joints, standard value at low stress (about) | 23 | 23 |
Sources
- Yaguchi, Kanai, Tamura: Temperature dependence of creep rupture life of long-term serviced Grade 91 steel, Frontiers in Materials 12 (2025) (accessed 2026-11-18)
Compiled by CASRAI from the sources above. Free to reuse under CC BY 4.0 with attribution.