Skip to main content
v2026.11,986 entries · CC-BY 4.0

S-N Curve: How to Read It, Endurance Limit and ASTM Test Standards

How to read an S-N (stress-life) curve: amplitude, R ratio, Basquin slope, endurance limit, and the scope limits of ASTM E466 and E739.

Written and maintained by CASRAI Editorial Board

Published

On this page

An S-N curve (stress-life curve, also called a Wöhler curve) plots the cyclic stress a material is subjected to against the number of cycles it survives before fatigue fracture. Stress amplitude goes on the vertical axis and cycles to failure, Nf, on a logarithmic horizontal axis. Lower stress amplitudes give longer lives, and for some metals the curve flattens into an endurance limit.

What an S-N curve plots

Fatigue is failure under time-varying loading. According to Stanford’s ME111 course handout on fatigue, it occurs at stresses well below the material’s yield strength and proceeds in three stages: crack initiation, crack propagation and final fracture. An S-N curve summarises how long a material lasts under a repeated, regular stress cycle. Each data point is one specimen tested at one stress level until it fractures (or until the test is stopped). The TU Delft materials science course (Materiaalkunde 1, chapter 9) describes the plot as cyclic stress amplitude against cycles to fracture Nf, with cycles to failure increasing as the amplitude decreases.

The curve is a property of a specific combination of material, specimen geometry, surface condition, loading mode and test conditions. It is not a single constant of the material. ASTM E466 says its test results are suitable for design only when the specimen test conditions realistically simulate service conditions, or when a methodology for accounting for service conditions is available and clearly defined.

Reading the curve: amplitude, mean stress and R

For a sinusoidal stress cycle, the Delft course defines the stress amplitude as σa = (σmax − σmin)/2 and the mean stress as σm = (σmax + σmin)/2. The stress ratio is R = σmin/σmax. An S-N curve is normally reported for one specified R: R = −1 means fully reversed loading with zero mean stress, and R = 0 means the stress cycles between zero and σmax.

Worked arithmetic illustration

This is an illustration of the formulas above, not test data. Suppose a cycle runs between σmax = +300 MPa and σmin = −100 MPa. Then σa = (300 − (−100))/2 = 200 MPa, σm = (300 + (−100))/2 = 100 MPa and R = −100/300 ≈ −0.33. A fully reversed cycle between +200 MPa and −200 MPa has the same amplitude of 200 MPa but σm = 0 and R = −1. The two cycles do not sit on the same S-N curve, because the mean stress differs. This is why a curve quoted without its R, or one that mixes amplitude with maximum stress on the vertical axis, cannot be compared like for like with another.

Basquin’s law and the log-log slope

In the high-cycle region, where stresses stay below yield, the Delft course gives Basquin’s law as Δσ · Nfb = C1, where b is small (0.07 to 0.13) and C1 is a material constant. Taking logarithms turns this into a straight line on log-log axes, which is why S-N data are usually plotted with a logarithmic life axis. For low-cycle fatigue, where plastic strain dominates, the same course gives the Coffin relation: plastic strain range = C2/Nfc, with c about 0.5. Stanford’s handout expresses the finite-life line between 103 and 106 cycles as S = aNb on log-log coordinates. Read the slope as follows: a small b means the allowable stress falls slowly as the required life grows by orders of magnitude.

Endurance limit, runouts and metals without one

The Delft course defines the endurance limit σe as the fatigue strength at 107 cycles: the stress amplitude, about a zero mean, below which fracture does not occur before at least 107 cycles. The Stanford handout lists the stress-life approach as seeking both the fatigue strength and the endurance limit, and gives a corrected endurance limit Sn = CL CG CS S′n, where the C factors correct for load type, stress gradient and surface condition.

Not every material shows a flat plateau. The Stanford handout lists copper alloys as having no endurance limit. For a material without one, a design life or a fatigue strength at a stated number of cycles has to be quoted instead. A test specimen that survives to the chosen cycle cutoff without failing is a runout: the test was stopped, and the specimen’s true life is unknown beyond that number.

How S-N data are generated and analysed: ASTM E466 and E739

Two ASTM practices frame most laboratory S-N work. ASTM E466 (Committee E08) is the standard practice for conducting force-controlled, constant-amplitude axial fatigue tests of metallic materials. ASTM E739 covers the statistical analysis of linear or linearised stress-life (S-N) and strain-life (ε-N) fatigue data. The checklist below shows what each one says about where its results are valid.

Question What the standard says Source
What loading does the test cover? Axial, force-controlled fatigue tests of metallic materials in the regime where strains are predominately elastic, on unnotched and notched specimens, with a constant-amplitude periodic forcing function in air at room temperature. ASTM E466-21, scope 1.1
Can it be used on whole parts? No. It is limited to specimens and does not cover full-scale components, structures or consumer products. ASTM E466-21, scope 1.2
What is it used to study? The effect of material, geometry, surface condition and stress on fatigue resistance for relatively large numbers of cycles. ASTM E466-21, 4.1
What must be reported? All material variables, testing information and procedures; hardness, cleanliness, grain size, surface residual stress and finish are named as nuisance variables. ASTM E466-21, 4.2
When are results suitable for design? Only when the test conditions realistically simulate service conditions, or a method of accounting for service conditions is clearly defined. ASTM E466-21, 4.3
Which curves can be fitted statistically? Only S-N and ε-N relationships reasonably approximated by a straight line, on appropriate coordinates, over a specific interval of stress or strain. ASTM E739-10, scope 1.1
Can the fitted line be extrapolated? Not recommended outside the interval of testing, nor to estimate life at an amplitude below about the fifth percentile (P ≈ 0.05). ASTM E739-10, scope 1.1

Because fatigue lives at a single stress level scatter widely, an S-N curve drawn through one specimen per level is weaker evidence than a fitted curve with a stated probability. Lifetime scatter is often handled with distributions such as the one covered in the CASRAI guide to Weibull analysis. Standards such as E466 and E739 can be searched in the ASTM compass service, described in the ASTM Compass guide.

Stress-life, strain-life and fracture mechanics compared

The S-N approach is one of three used in fatigue design. The data table below compares them as presented in the Stanford ME111 handout and the Delft course. In short, stress-life is most useful for high-cycle fatigue under regular loading; strain-life suits low-cycle fatigue and crack initiation; and linear elastic fracture mechanics (LEFM) describes crack propagation. The Delft course also separates initiation-controlled life, for an undamaged sample, from propagation-controlled life, where a crack is already present; these call for different design approaches.

Mean stress is handled separately from the base curve. The Stanford handout uses Goodman and Gerber lines to account for it, and defines the factor of safety as Nf = Sf/σa for finite life or Se/σa for infinite life. Environmental effects are outside E466’s room-temperature-air scope; for corrosion-assisted cracking see the guide to stress corrosion cracking. For how loads become stresses in a part, see solid mechanics. Process routes that change porosity and therefore fatigue behaviour, such as hot isostatic pressing, are tested against the same kind of curves.

Where it matters for test labs

For a materials-testing lab, the practical content of the sources above reduces to a short reporting checklist:

  • State whether the vertical axis is stress amplitude or maximum stress, and give R and the mean stress.
  • State the cycle count at which a test is stopped and treated as a runout (107 is the cycle count in the Delft definition of the endurance limit).
  • Record specimen geometry, notch condition, surface finish, hardness, cleanliness, grain size and residual stress (the nuisance variables in E466 section 4.2).
  • State the environment and temperature, since E466 covers air at room temperature only.
  • Do not extrapolate a fitted line beyond the tested stress interval or into the lowest-probability tail (E739).
  • Do not read specimen curves as component lives unless service conditions are accounted for (E466 4.3).

Common misunderstandings

An S-N curve gives the life of a part

It gives the life of a specimen under the stated test conditions. E466 explicitly excludes full-scale components and structures from its scope.

Every material has an endurance limit

Stanford’s handout lists copper alloys as having no endurance limit, so a plateau cannot be assumed for every material. Delft’s definition of the endurance limit is itself tied to a stated cycle count (107).

Stress below the yield strength is safe

Stanford’s handout notes that fatigue failure occurs at stress well below the yield strength.

The S-N curve covers cracks already present

Stress-life is an initiation-oriented approach for undamaged material; once a crack exists, the Delft course says a propagation-based approach is needed.

FAQ

What does S-N stand for?

Stress (S) versus number of cycles to failure (N). The curve is also called a stress-life or Wöhler curve.

What is the endurance limit on an S-N curve?

Per the TU Delft course, the fatigue strength at 107 cycles: the stress amplitude (about zero mean) below which fracture does not occur before at least 107 cycles.

Why is the horizontal axis logarithmic?

Fatigue lives span many orders of magnitude, and Basquin’s law becomes a straight line on log-log axes.

Do all metals have an endurance limit?

No. Stanford’s ME111 handout lists copper alloys as having none, so a fatigue strength at a stated number of cycles is quoted instead.

Which standards cover S-N testing?

ASTM E466 for force-controlled axial fatigue testing of metallic specimens and ASTM E739 for the statistical analysis of S-N and ε-N data.

Sources

Data: Fatigue design approaches: stress-life, strain-life and fracture mechanics

Comparison of the three fatigue approaches (stress-life, strain-life, linear elastic fracture mechanics) by the regime or stage each addresses, compiled from a university lecture handout and a university materials course.

Fatigue design approaches: stress-life, strain-life and fracture mechanics
ApproachRegime or stage addressedTypical outputs or use
Stress-life (S-N)High-cycle fatigue (N > 10^3) with regular loadingFatigue strength and endurance limit
Strain-lifeLow-cycle fatigue and crack initiationLife from strain range (Coffin relation for plastic strain)
Linear elastic fracture mechanicsCrack propagation (a crack is present)Propagation-controlled life of a cracked part

Sources

Compiled by CASRAI from the sources above. Free to reuse under CC BY 4.0 with attribution.

Follow CASRAI

Research-administration guidance, standards updates and independent tool reviews.

Ask CASRAI · full access

Ask about S-N Curve: How to Read It, Endurance Limit and ASTM Test Standards

Full access: large monthly usage, up to 10 source passages behind each answer, and MCP and API access for Claude Code, Codex and other CLIs. Cancel any time.

An AI assistant for research: funder rules, compliance, methods and publishing. It links the sources behind its answers and labels answers that come from a web search.

Answers draw on CASRAI's guides and dictionary plus the federal and funder documents we index: Federal Register, Grants.gov, Regulations.gov and UKRI.

Works on this site and inside Claude, Cursor and the AI tools you already use.

Everything CASRAI publishes — this page, the dictionary, the guides and the news — stays open to read, with no account and no card.

Referenced across the research world

University of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logoUniversity of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logo
  • University of Cambridge logo
  • Columbia University logo
  • Crossref logo
  • University of Edinburgh logo
  • Harvard University logo
  • University of Oxford logo
  • Princeton University logo
  • Stanford School of Medicine logo
  • University College London logo
  • ORCID logo

View CASRAI adoption →