Skip to main content
v2026.11,986 entries · CC-BY 4.0

Salt Spray Test: How ASTM B117 Works and What Results Mean

How a salt spray (salt fog) test works under ASTM B117, what the standard leaves to the specification, and how to read the results.

Written and maintained by CASRAI Editorial Board

Published · Last updated

On this page

Short answer

A salt spray test (also called a salt fog test) exposes metal or coated-metal specimens to a continuously generated saltwater mist inside a closed chamber, so that relative corrosion resistance can be compared under controlled, repeatable conditions. The best-known method is ASTM B117, and ISO 9227 is the widely used international counterpart. It ranks samples against each other; on its own it does not tell you how many years a part will last outdoors.

Definition and scope

ASTM B117 (the edition listed on the ASTM store as of 2026-11-13 is B117-26, from committee G01 on corrosion of metals) covers the apparatus, the procedure and the conditions needed to create and maintain a salt spray environment. Its stated purpose is to supply a controlled corrosive environment that yields relative corrosion-resistance information for metals and coated metals tested in a given chamber. The apparatus is described in an appendix of the standard.

The scope statement is as important for what it leaves out. According to the ASTM abstract, B117 does not prescribe the type of specimen, the length of exposure for a given product, or how the results are to be interpreted. Those decisions belong to the product specification, customer requirement or test plan that calls up the method. Anyone writing a laboratory procedure around the test needs to know this split, because the phrase “passed ASTM B117” is incomplete without the hours, the specimen preparation and the acceptance criterion that went with it.

Typical users are automotive, construction, aerospace, consumer-goods and electronics manufacturers and paint and coating producers (Q-Lab lists these industries). In a research setting the test is a screening tool for coatings, platings, conversion layers and passivation treatments; see the related guides on corrosion-protective coatings and passivation of stainless steel.

How the test is run in practice

The conditions below are those published by Q-Lab (an instrument maker) and Infinita Lab (a testing laboratory) for the neutral salt spray method in B117. They are summarised here for orientation; the standard itself is the controlling document.

  • Solution: 5% sodium chloride in distilled or deionized water, with pH at 6.5 to 7.2 measured at the collection temperature. If the pH is off, it is adjusted with dilute acetic acid or sodium hydroxide.
  • Chamber temperature: 35 °C, with a tolerance of ±2 °C.
  • Fog: compressed air and salt solution are fed to a nozzle that atomizes the solution continuously. Fog collectors verify the rate: 1 to 2 mL per hour, measured over an 80 cm² horizontal collection area (a 10 cm funnel).
  • Specimen placement: specimens are cleaned beforehand, held roughly 15 to 30 degrees from vertical, and kept from touching each other or the chamber walls. Dissimilar materials whose corrosion products could contaminate neighbouring specimens should not share a cabinet.
  • Coated specimens: these are often scribed through to the substrate so that corrosion creep from the cut can be assessed.

What the standard decides and what the specification decides

Because B117 is an environment standard rather than a product standard, test reports are only comparable when the second column below is also stated. The split is drawn from the ASTM abstract and the Infinita Lab guide.

Decided by the test method (B117) Decided by the product specification, customer or test plan
Apparatus and chamber construction Specimen type, size and surface preparation
Salt solution concentration, pH and water quality Exposure duration in hours
Chamber temperature and fog collection rate Acceptance and rejection criteria
General rules for specimen arrangement Which rating method is used to evaluate the result

Typical rating methods named by Infinita Lab for evaluating exposed specimens are ASTM D1654 (corrosion creep from a scribe), ASTM D714 (degree of blistering) and ASTM D610 (degree of rusting), often with photographic documentation.

Neutral, acetic acid and copper-accelerated tests, and cyclic variants

Neutral salt spray (NSS) is only one of several fog tests. ISO 9227 defines NSS, acetic acid salt spray (AASS) and copper-accelerated acetic acid salt spray (CASS), and ASTM G85 defines modified tests, some of which cycle between fog, dry and humid phases. The data table below this article compares the solution, pH, temperature and cycle of each as tabulated by the testing laboratory Micomlab. Use it to see how quickly the tests diverge from plain B117: the acidified tests run at pH 2.8 to 3.3 rather than neutral, CASS runs hotter at 50 °C and adds copper chloride, and the G85 cyclic tests alternate fog with dry-air or humid periods.

Infinita Lab also points to cyclic methods such as SAE J2334 and GMW14872 as alternatives used where steady fog is considered too unrealistic. Choosing among these is a specification decision, not a laboratory preference.

Reading the results and their limits

ASTM states in the B117 significance section that results from the test used alone have seldom been correlated with performance in natural environments, and that correlation or extrapolation is not always predictable. It advises considering such links only where long-term atmospheric exposures support them. Reproducibility also depends on specimen type, the evaluation criteria and control of operating variables; ASTM notes that similar specimens in different chambers under nominally similar conditions have shown variability, and recommends enough replicates to judge scatter.

Q-Lab lists further limits: the constant 35 °C fog does not reproduce humidity and temperature swings, complex salts or pollutants; a neutral solution can miss corrosion driven by acid or alkaline conditions; the test is focused on surface behaviour; and a coating that survives may still fail under UV or cyclic outdoor exposure. Infinita Lab summarises the position as a quality screen and comparative tool, not a service-life predictor, and notes there is no universal conversion from chamber hours to years in service.

Checklist for planning a salt spray test

Each item traces to the sources listed at the end of the page.

  1. Write down the governing standard and edition (for example B117-26 or the ISO 9227 version named by the customer) and the specification that sets duration and acceptance. B117 does not supply these.
  2. Define the specimen type, geometry and cleaning method, and whether coated specimens are scribed.
  3. Decide the number of replicates up front; ASTM ties reproducibility to replication and to control of operating variables.
  4. Prepare solution from distilled or deionized water at the specified concentration, and check pH at collection temperature.
  5. Check chamber temperature and measure fog collection (1 to 2 mL/h over the stated area) with collectors before relying on a run.
  6. Position specimens at the stated angle without contact with each other or the walls, and keep dissimilar metals that could cross-contaminate in separate runs.
  7. Name the rating method (for example D1654, D714 or D610) and record photographs at each inspection.
  8. Report the result as relative performance in that chamber and test type, not as a service-life estimate. For laboratory write-ups, a standard operating procedure can hold these decisions in one controlled document.

Common misunderstandings

“A part that passes 1,000 hours will last a set number of years”

No source supports a fixed hours-to-years conversion. Infinita Lab states there is none, and ASTM cautions that correlation to natural exposure is not reliably predictable from the salt spray result alone.

“B117 sets the pass mark”

It does not. Duration and acceptance come from the product specification or customer requirement.

“All salt spray tests are the same”

Neutral, acetic acid, copper-accelerated and cyclic tests differ in pH, temperature and cycle, and results from one are not interchangeable with another. Corrosion modes such as stress corrosion cracking are also outside what a surface-focused fog test is designed to show.

“The same coating gives the same result in any chamber”

ASTM reports variability between chambers even under nominally similar conditions, which is why chamber verification, replicates and clear reporting matter. The same logic applies to replicates in other lab disciplines.

Frequently asked questions

What is a salt spray test?

A corrosion test in which specimens sit in a closed chamber filled with a continuously atomized saltwater fog, used to compare the corrosion resistance of metals and coatings under controlled conditions.

What is ASTM B117?

The ASTM standard that covers the apparatus, procedure and conditions for creating and maintaining a salt spray (fog) environment. It does not set specimen type, exposure time or interpretation of results.

What temperature and salt concentration are used?

For the neutral test in B117, published summaries give 35 °C (±2 °C) and 5% sodium chloride at pH 6.5 to 7.2.

How long does a salt spray test last?

It depends on the specification that calls for the test; B117 itself does not fix a duration.

What is the difference between ASTM B117 and ISO 9227?

Both are salt spray methods. ISO 9227 covers neutral (NSS), acetic acid (AASS) and copper-accelerated (CASS) tests; see the data table for the tabulated differences in solution, pH and temperature.

Can salt spray results predict service life?

No. Sources describe the test as a relative, comparative screen rather than a service-life predictor.

Sources

Data: Salt fog corrosion test types: solution, pH, temperature and cycle (ASTM B117, ASTM G85, ISO 9227)

Compares the neutral, acidified, copper-accelerated and cyclic salt fog test types by solution, pH, chamber temperature and cycle, as tabulated by a corrosion testing laboratory and cross-checked against Q-Lab for B117.

Period covered: 2026.

Salt fog corrosion test types: solution, pH, temperature and cycle (ASTM B117, ASTM G85, ISO 9227)
Test typeSolutionpHChamber temperature (°C)Cycle
ASTM B117 (neutral salt spray)5% NaCl (±1%)6.5-7.235 ±2Continuous fog
ISO 9227 NSSSodium chloride6.5-7.235 ±2Continuous fog
ISO 9227 AASSSodium chloride with acetic acid3.1-3.335 ±2Continuous fog
ISO 9227 CASSSodium chloride with 0.26 g/L CuCl2·2H2O3.1-3.350 ±2Continuous fog
ASTM G85 A1NaCl with acetic acid3.1-3.335 ±2Continuous fog
ASTM G85 A25 ± 1% NaCl2.8-3.049 ±2 (fog phase)0.75 h fog, 2 h dry air purge, 3.25 h humidity
ASTM G85 A3Synthetic sea salt2.8-3.024 to 35 or 49 ±2 (fog phase)0.5 h fog, 1.5 h humidity
ASTM G85 A50.35% (NH4)2SO4 + 0.05% NaCl5.0-5.435 ±1.51 h fog, 1 h dry

Sources

Compiled by CASRAI from the sources above. Free to reuse under CC BY 4.0 with attribution.

Follow CASRAI

Research-administration guidance, standards updates and independent tool reviews.

Ask CASRAI · full access

Ask about Salt Spray Test: How ASTM B117 Works and What Results Mean

Full access: large monthly usage, up to 10 source passages behind each answer, and MCP and API access for Claude Code, Codex and other CLIs. Cancel any time.

An AI assistant for research: funder rules, compliance, methods and publishing. It links the sources behind its answers and labels answers that come from a web search.

Answers draw on CASRAI's guides and dictionary plus the federal and funder documents we index: Federal Register, Grants.gov, Regulations.gov and UKRI.

Works on this site and inside Claude, Cursor and the AI tools you already use.

Everything CASRAI publishes — this page, the dictionary, the guides and the news — stays open to read, with no account and no card.

Referenced across the research world

University of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logoUniversity of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logo
  • University of Cambridge logo
  • Columbia University logo
  • Crossref logo
  • University of Edinburgh logo
  • Harvard University logo
  • University of Oxford logo
  • Princeton University logo
  • Stanford School of Medicine logo
  • University College London logo
  • ORCID logo

View CASRAI adoption →