Zerodur: Zero-Expansion Glass-Ceramic, CTE Classes and Limits

What Zerodur is, what its expansion classes really mean, how CTE is measured, and which heat exposures change it.

Written and maintained by CASRAI Editorial Board

Published

On this page

Zerodur is a trademarked lithium aluminum silicon oxide glass-ceramic made by SCHOTT, sold for its extremely low thermal expansion. Its coefficient of thermal expansion (CTE) is held within a small tolerance around zero, measured as a mean over 0 °C to 50 °C, so a part stays almost the same size when the room warms or cools. That is why it is used for telescope mirror blanks, metrology frames and other optics where shape stability matters.

Definition and scope

SCHOTT describes Zerodur as an inorganic, non-porous glass-ceramic with a very low rate of imperfections, transparency to visible light, and thermal expansion that is homogeneous throughout the entire volume of a part. The company says it can be supplied from a few centimeters up to about 4 m in size, that its low-expansion properties stay homogeneous up to 4.25 m and beyond, and that surfaces with sub-nanometre roughness are achievable (SCHOTT product page, read 2026-11-18). It has been on the market for over 50 years.

The name covers a family rather than a single number. SCHOTT’s technical data defines expansion classes, homogeneity guarantees by blank weight, inclusion and bulk-stress quality levels, and two variants, ZERODUR K20 and ZERODUR TAILORED. This page explains how those pieces fit together for researchers and lab staff who read a data sheet or a mirror specification that names the material. It is a materials explainer, not a purchasing guide.

How the near-zero expansion arises

SCHOTT’s technical information note TIE-37 explains the mechanism. Zerodur contains about 70-78 weight percent crystalline phase with a high-quartz structure, with an average crystal size of about 50 nm, embedded in a residual glass phase. The crystal phase has a negative linear thermal expansion, while the glass phase has a positive one, so the two largely cancel over the working temperature range (SCHOTT TIE-37, read 2026-11-18).

The same note describes the route to that structure. The melt is cast into molds and cooled to room temperature in annealing ovens in a controlled way over several weeks. At that stage the glassy raw casting still has a CTE of about +3 × 10-6 K-1. The pre-crystallized outer layers are removed, and the material is then ceramized: a controlled heat treatment that grows the crystals, which can take up to several months depending on part size. CTE samples are taken from the final material to estimate its final CTE and homogeneity.

What “zero expansion” means in a specification

The number is a mean over 0 °C to 50 °C

The default CTE in SCHOTT’s data is written CTE (0 °C; 50 °C) and is the linear mean coefficient of thermal expansion between 0 °C and 50 °C. Zerodur is optimized for that range. A class tolerance such as 0 ± 0.020 × 10-6/K therefore says that the mean expansion over that interval falls within the band; it does not say that the length is unchanged at every temperature. SCHOTT also states that, on request, expansion class 0 or better can be optimized for a customized temperature range, which is what the TAILORED variant is.

Expansion classes

SCHOTT lists five expansion classes plus TAILORED, all as mean CTE (0 °C; 50 °C), in units of 10-6/K:

  • Expansion Class 2: 0 ± 0.100
  • Expansion Class 1: 0 ± 0.050
  • Expansion Class 0: 0 ± 0.020
  • Expansion Class 0 SPECIAL: 0 ± 0.010
  • Expansion Class 0 EXTREME: 0 ± 0.007
  • TAILORED: ± 0.020 (± 0.010 on request), optimized for the application temperature

The maximum application temperature stated for standard Zerodur is 600 °C. The data table below places these tolerances next to the other quantities discussed on this page so they can be compared in one unit.

Homogeneity is a separate guarantee

Homogeneity is not the same as the class. SCHOTT evaluates it by measuring CTE samples distributed through the blank and taking the difference between the highest and lowest value. The guaranteed limits depend on blank weight: below 0.03 × 10-6/K up to 18 tons, below 0.02 up to 6 tons and below 0.01 up to 0.3 tons. SCHOTT shows a 1.5 m blank with a measured homogeneity of 0.004 × 10-6/K as an example.

TIE-37 adds statistics from more than 200 astronomical mirror blanks of 1 to 2 m diameter made at SCHOTT. It reports that 95% of standard blanks in the 1 to 2 m class show homogeneity better than 0.010 × 10-6/K. In its most extensive single-blank measurement, 111 samples from a 1554 mm diameter, 345 mm thick blank gave a total peak-to-valley variation of 0.0064 × 10-6/K.

How the CTE is measured

TIE-37 describes a modified push-rod dilatometer. The sample is 100 mm long and 6 mm in diameter, the sample holder and push rod are made of titanium silicate glass, temperature is read with a platinum resistance thermometer, and the instrument is calibrated against a titanium silicate reference sample measured at the Physikalisch-Technische Bundesanstalt (PTB) with an interferometer system, to an absolute accuracy of 0.005 × 10-6/K.

The note gives two setups for CTE (0 °C; 50 °C): the standard dilatometer has an accuracy of 0.0100 and a 95% repeatability of 0.0050, and the improved dilatometer, which replaces the LVDT with an interferometer, has an accuracy of 0.0062 and a repeatability of 0.0012, all in 10-6/K. The practical consequence is worth stating plainly: the tightest classes are only a few times larger than the best published measurement accuracy, so the class is a statement about a measurement as well as about the glass. TIE-37 also notes that the CTE depends on temperature and time history, so values derived from thermal-length-change curves are less accurate than those from the 0 °C to 50 °C method.

Thermal history and handling limits

The most common misreading of “zero expansion” is that the material is indifferent to temperature excursions. TIE-37 identifies three temperature ranges in which dimensional stability can change:

  • Above 700 °C (ceramization range): ceramization continues and the CTE changes irreversibly for all temperature ranges.
  • About 130 °C to 320 °C (upper relaxation range): in quench tests on well-annealed samples, no change in CTE (0 °C; 50 °C) was seen up to about 130 °C, and the CTE after quenching rose with the starting temperature until it saturated at 320 °C. Faster cooling than the original anneal rate shifts the CTE: cooling from 300 °C at 30 K/h gave a relative elongation of 14 × 10-6 for a sample originally annealed at 1 K/h. The effect is reversible by heating above 320 °C and cooling at the original rate, and is stable at room temperature.
  • About -70 °C to +40 °C (lower relaxation range): thermal cycling produces a reversible hysteresis in the length-versus-temperature curve of the order of 10-6 relative length change, which relaxes in a relatively short time even at fairly low temperatures.

The note also reports a long-term test: a 400 mm bar held at 20 °C at PTB Braunschweig from September 1973 for about 10 years showed a continuous, monotone decrease in length, often called aging. For mirror coating, TIE-37 says the elevated temperatures are short and affect only a thin layer, and that experience shows a negligible effect on the surface figure.

At low temperatures, SCHOTT’s own measurements go down to about -180 °C (93 K). For lower temperatures TIE-37 cites other institutes: a maximum CTE of -0.4 × 10-6/K at about 20 K, and a test in which two 300 mm parabolic mirrors cooled from room temperature to 130 K showed no significant distortion.

Variants: ZERODUR K20 and TAILORED

ZERODUR K20 is the high-temperature version. SCHOTT gives its mean CTE as 2.4 × 10-6/K between 20 °C and 700 °C, 2.2 between 20 °C and 300 °C and 1.6 between 0 °C and 50 °C, with a maximum application temperature of 850 °C. The contrast with standard Zerodur is the point: K20 is not a near-zero-expansion grade at room temperature but a variant designed to withstand higher temperatures.

TAILORED moves the zero crossing of the expansion curve to a chosen temperature. TIE-37 explains that the thermal-length-change curve can be adjusted so the CTE passes through exactly zero at a given temperature under defined conditions, and shows two example curves with zero crossings at different temperatures.

Inclusions and bulk stress

Besides expansion, SCHOTT’s data defines optical-quality levels. The main inclusions in Zerodur are bubbles, and during inspection all inclusions larger than 0.3 mm in diameter are counted. There are six inclusion quality levels (Standard and Classes 4 to 0), with an average number of inclusions per 100 cm3 of 5.0 for Standard and 1.0 for Class 0, plus limits on the maximum diameter of individual inclusions that depend on part size. Bulk stress birefringence is specified in nm/cm, again by part size. Individual specifications can be requested.

Where it matters for labs and instrument decisions

SCHOTT names ground-based and space astronomy as headline uses: the Extremely Large Telescope, and the European Space Agency’s LISA Pathfinder mission, which SCHOTT describes as having Zerodur at its core. TIE-37 lists mirror-blank projects including the Keck telescopes, the Hobby-Eberly Telescope and the Gran Telescopio Canarias, and a SCHOTT conference paper records that the company marked 100 years of delivering astronomical mirror blanks in 2003. The product page also names low gas permeability as the property relevant to He-Ne ring laser gyroscopes.

For a research group, the useful output of the sources above is a checklist of what a Zerodur part description has to pin down. This is an editorial reading of the quantities SCHOTT defines, not a procurement rule:

  1. Which expansion class, and over which temperature interval the CTE is stated (0 °C to 50 °C by default).
  2. Whether blank-level homogeneity is specified, and for which weight class.
  3. Which inclusion and bulk-stress quality levels apply, by part size.
  4. The thermal exposure the part will see: anything above about 130 °C with a fast cool-down is in the range where TIE-37 reports reversible CTE shifts, and above 700 °C the changes are irreversible.
  5. Whether the application temperature is far from 20 °C, which is when the TAILORED variant or the lower relaxation hysteresis becomes relevant.

For neighbouring material families, see CASRAI’s guides on alumina ceramics and refractory ceramics, and for optical systems where thermal stability of mirrors matters, adaptive optics and optics and photonics. Discipline context is on the materials science page.

Common misunderstandings

  • “Zero expansion at every temperature.” The classes are mean values over 0 °C to 50 °C; the length-versus-temperature curve is not flat.
  • “A higher class means a different material.” The classes describe the tolerance band of the measured mean CTE; homogeneity, inclusions and bulk stress are separate quality levels.
  • “It is unaffected by heat.” Above about 130 °C, cooling rate can shift the CTE reversibly, and above 700 °C the change is permanent (SCHOTT TIE-37).
  • “Zerodur is a generic term.” It is a SCHOTT trademark for this specific glass-ceramic.
  • “K20 is a lower-expansion version.” K20 is the high-temperature variant, with a mean CTE of 1.6 × 10-6/K at 0 °C to 50 °C.

Sources

Data: ZERODUR expansion tolerances, homogeneity limits and CTE measurement accuracy

One table that puts SCHOTT's published Zerodur expansion-class tolerances, blank-weight homogeneity limits, K20 mean CTE values and the TIE-37 dilatometer accuracy and repeatability figures in a single unit (10^-6 per kelvin) so they can be compared directly. Compiled from SCHOTT's product technical details and technical information note TIE-37.

ZERODUR expansion tolerances, homogeneity limits and CTE measurement accuracy
QuantityValue (10^-6 per K)Kind of figureCondition or definition
Expansion Class 20.1CTE tolerance, classMean CTE 0-50 C, 0 +/- value
Expansion Class 10.05CTE tolerance, classMean CTE 0-50 C, 0 +/- value
Expansion Class 00.02CTE tolerance, classMean CTE 0-50 C, 0 +/- value
Expansion Class 0 SPECIAL0.01CTE tolerance, classMean CTE 0-50 C, 0 +/- value
Expansion Class 0 EXTREME0.007CTE tolerance, classMean CTE 0-50 C, 0 +/- value
TAILORED0.02CTE tolerance, variantOptimized for application temperature; 0.010 on request
Homogeneity limit, blanks up to 18 tons0.03Guaranteed upper limitHighest minus lowest CTE across samples, 0-50 C
Homogeneity limit, blanks up to 6 tons0.02Guaranteed upper limitHighest minus lowest CTE across samples, 0-50 C
Homogeneity limit, blanks up to 0.3 tons0.01Guaranteed upper limitHighest minus lowest CTE across samples, 0-50 C
Dilatometer accuracy, standard setup0.01Measurement accuracyCTE (0 C; 50 C), push-rod dilatometer
Dilatometer accuracy, improved setup0.0062Measurement accuracyCTE (0 C; 50 C), interferometric readout
Dilatometer repeatability (95%), standard0.005Measurement repeatabilityCTE (0 C; 50 C)
Dilatometer repeatability (95%), improved0.0012Measurement repeatabilityCTE (0 C; 50 C)
ZERODUR K20 mean CTE, 20-700 C2.4Mean CTE valueHigh-temperature variant, max application temperature 850 C
ZERODUR K20 mean CTE, 20-300 C2.2Mean CTE valueHigh-temperature variant
ZERODUR K20 mean CTE, 0-50 C1.6Mean CTE valueHigh-temperature variant

Sources

Compiled by CASRAI from the sources above. Free to reuse under CC BY 4.0 with attribution.

Follow CASRAI

Research-administration guidance, standards updates and independent tool reviews.

Ask CASRAI · full access

Ask about Zerodur: Zero-Expansion Glass-Ceramic, CTE Classes and Limits

Full access: large monthly usage, up to 10 source passages behind each answer, and MCP and API access for Claude Code, Codex and other CLIs. Cancel any time.

An AI assistant for research: funder rules, compliance, methods and publishing. It links the sources behind its answers and labels answers that come from a web search.

Answers draw on CASRAI's guides and dictionary plus the federal and funder documents we index: Federal Register, Grants.gov, Regulations.gov and UKRI.

Works on this site and inside Claude, Cursor and the AI tools you already use.

Everything CASRAI publishes — this page, the dictionary, the guides and the news — stays open to read, with no account and no card.

Referenced across the research world

University of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logoUniversity of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logo
  • University of Cambridge logo
  • Columbia University logo
  • Crossref logo
  • University of Edinburgh logo
  • Harvard University logo
  • University of Oxford logo
  • Princeton University logo
  • Stanford School of Medicine logo
  • University College London logo
  • ORCID logo

View CASRAI adoption →