Binder Jetting: How the Process Works and Its Limits

Binder jetting explained: the print, cure, depowder, debind and sinter workflow, with parameters from two metal studies and the limits authors report.

Written and maintained by CASRAI Editorial Board

Published

On this page

Binder jetting is an additive manufacturing process in which a liquid bonding agent (the binder) is selectively deposited onto a bed of powder, layer by layer, so that the powder particles stick together into a shape. The printed “green” part is weak and must usually be cured, cleared of loose powder and, for metals, debound and sintered before it reaches useful density. This guide explains the workflow, the post-processing that decides the result, and where the process fits against other powder-based routes.

Definition and scope

The ISO/ASTM 52900 terminology standard defines binder jetting as an “additive manufacturing process in which a liquid bonding agent is selectively deposited to join powder materials”, as quoted in a 2022 review in Polymers (Azlin et al., Table 2). The defining feature is that the binder, not a laser or electron beam, does the joining during printing. The same review describes it as a cold process that does not involve a heating element to bind the material, and notes that this makes the printing step energy-efficient because no heat is needed to fuse the layer.

That printing-step description is easy to over-read. Most binder-jetted parts are not finished when printing stops. A 2025 study of H13 tool steel in Materials (Widomski et al.) describes three key stages for the metal route: 3D printing, debinding (binder removal) and sintering. A 2022 review of binder jetting for pharmaceuticals in Pharmaceutics adds depowdering, the removal of loose powder from the green part, and optional infiltration as a strengthening step. Binder jetting is therefore best understood as a process chain that starts with a cold printing step, not as a single machine operation.

Scope for this page: the process principle, the workflow, the variables that the cited studies report, and the limits those authors state. It does not recommend equipment, suppliers or settings. Where parameters appear, they belong to one study and one material, and they are not general rules.

How binder jetting works in practice

Layer by layer: powder and binder

The Pharmaceutics review describes the printing loop as a computer-controlled roller that spreads a fresh powder layer, followed by a drop-on-demand printhead that deposits binder onto the regions that will become the part. Printheads can be thermal bubble or piezoelectric, and the binder can be aqueous, organic or a mixture. The platform then lowers and the cycle repeats. The Azlin review summarises the same sequence as powder deposition to produce the layers, binder application and post-processing.

Because unbound powder surrounds the part throughout the build, the same review notes that no support structures are needed, and that full-colour printing is possible in principle. The cost of that freedom is that the part has not been compacted: the review lists a rough surface and lower mechanical strength among the limitations.

Worked example: the stages for a metal part

The most detailed parameter set in the sources cited here comes from the H13 tool steel study. In that work the printing stage used a layer thickness of 70 µm and a binder saturation of 80%, with drying at 35 °C and 10 to 30 seconds per layer. Thermal debinding was a single stage between 500 and 800 °C. Sintering ran at 1310 °C, with a heating rate of 50 °C per hour and a 4-hour hold in argon. The authors report a sintering shrinkage of 16 ± 2% in each of the X, Y and Z directions.

A second metal example, a 2016 data article in Data in Brief on alloy 625 (Mostafaei et al.), used an ExOne M-Flex printer with 100 µm layers and 10 × 10 × 5 mm coupons. Green parts were cured at 175 °C, then sintered between 1225 and 1300 °C for 4 hours in vacuum, packed in an alumina powder bed. The data table below puts the two studies side by side so the stage parameters can be compared directly; every figure in it is reported by the study named in its row.

Depowdering and strengthening

Depowdering is its own step. The Pharmaceutics review defines it as removal of loose powder within the green specimen, and states that poor powder flowability can hinder removal of powder from pores. Infiltration, the filling of the printed structure’s pores with a second material, is described there as a way to strengthen a green part, with a plaster print infiltrated with epoxy given as an example. The Azlin review gives a ceramic-and-polymer example: a calcium sulfate hemihydrate scaffold converted to biphasic calcium phosphate and infiltrated with polycaprolactone, with polycaprolactone loading above 40%.

Materials and process variables

Metal, ceramic, polymer-based and composite powders

The cited studies cover several material families, and the binder-jetting principle is the same in each: H13 tool steel and alloy 625 (metals), calcium sulfate and calcium phosphate scaffolds (ceramics), gypsum with sisal fibre (a composite) and cellulose-based food powders. The families differ in what comes after printing. Metals are debound and sintered; the scaffold example is chemically converted and then infiltrated; the pharmaceutical review stresses that organic binders call for residual-solvent checks, citing the ICH Q3C guideline. Fibre-filled powders have a specific drawback in the Azlin review: the fibres caused a loss of strength in the green parts, and producing multiple materials within one component remains restricted.

Powder size, layer thickness and powder shape

The Pharmaceutics review reports that a smaller average particle size gives higher resolution, that a thicker powder layer reduces mechanical strength, and that in cited studies at a 50 µm layer thickness most particles were pushed off the platform. Layer thickness and particle size therefore have to be considered together rather than minimised independently.

Powder shape matters for the final density. In the alloy 625 data article, gas-atomised powder was spherical with an average size of 32 µm, while water-atomised powder was irregular with an average size of 34.5 µm and more internal porosity. Under the study’s conditions the highest relative density reached about 95% for water-atomised powder (sintered at 1270 °C) and about 99.2% for gas-atomised powder (1285 °C). The two powders had almost the same average size, so the difference points to morphology and internal porosity rather than size. This is one alloy on one machine, so it should be read as a demonstration that powder choice can matter, not as a universal ranking. For how powder is specified and sourced more broadly, see the guide to metal powder for 3D printing.

Binder jetting compared with other powder-based routes

The H13 tool steel paper compared binder jetting with laser powder bed fusion (LPBF), directed energy deposition (DED) and fused deposition of metals and sintering (FDMS) in its Table 3. The figures below are that study’s, for that steel, and should not be generalised to other alloys or machines.

  • Density: LPBF 99.9%, DED above 99.9%, binder jetting 99.3%, FDMS 94% and 90.7% in two reported entries.
  • Deposition rate: binder jetting 5.5 kg/h, against 1 to 2 for DED, 1.5 to 3 for FDMS and 0.1 to 0.5 for LPBF.
  • Accuracy: rated high for binder jetting and LPBF, medium for DED.

The authors describe binder jetting as requiring one of the most expensive printing systems on the market and justify it only for high-precision, small-series production, and only if large-scale orders are available. That is the authors’ conclusion about their study, not a purchasing rule. The sintering route also links binder jetting to older powder technologies: see the guides on powder metallurgy and metal injection moulding, which share the binder-removal and sintering logic, and on hot isostatic pressing, a densification step that is a separate process from binder jetting itself.

Where it matters for laboratories and supply decisions

  • Powder specification: particle size, shape and flowability affect resolution, depowdering and final density in the sources above, so powder is a controlled input, not a commodity.
  • Shrinkage planning: a reported 16 ± 2% linear sintering shrinkage in the H13 study means a printed design must be scaled to the sintered target size, and the variation must be accepted within tolerances.
  • Furnace and atmosphere: the metal examples used argon or vacuum sintering above 1200 °C, so the thermal equipment is part of the system, not an afterthought.
  • Binder chemistry: in pharmaceutical applications, organic binders require residual-solvent checks, and the review says binder jetting is still in its infancy in pharmaceutical manufacturing.
  • Handling of loose powder: depowdering is a defined step in the workflow, and the pharmaceutical review notes that poor flowability can hinder it.

For wider context on the field, additive manufacturing sits with other manufacturing practice in the America Makes guide, which describes a US additive manufacturing institute.

Common misunderstandings

“Binder jetting is a cold process, so the part comes out finished”

Only the printing step is cold. The H13 study needed thermal debinding at 500 to 800 °C and sintering at 1310 °C, and the pharmaceutical review treats the printed part as a green specimen.

“Green parts are as strong as the final part”

The Pharmaceutics review ties the lack of a compaction step to lower mechanical strength, and the Azlin review reports fibres reducing green strength further. Metal parts gain their strength and density in sintering; in the H13 study as-printed hardness was about 235 HV0.5, rising to about 500 after tempering at 550 °C and 620 to 680 after quenching.

“Binder jetting needs supports like other additive processes”

The surrounding powder bed supports the part, so no support structures are needed according to the pharmaceutical review.

“One set of parameters works for every powder”

The parameters in these sources are tied to one alloy and one machine. Even two powders of the same alloy and similar mean size sintered to different densities in the alloy 625 data.

Sources

  • Azlin et al., “3D Printing and Shaping Polymers, Composites, and Nanocomposites: A Review”, Polymers 14(1):180, 2022 (cites ISO/ASTM 52900). https://pmc.ncbi.nlm.nih.gov/articles/PMC8747384/ (read 2026-11-14)
  • Widomski et al., “Comparative Study of Different Additive Manufacturing Methods for H13 Tool Steel”, Materials 18(23):5299, 2025. https://pmc.ncbi.nlm.nih.gov/articles/PMC12692884/ (read 2026-11-14)
  • “The Application and Challenge of Binder Jet 3D Printing Technology in Pharmaceutical Manufacturing”, Pharmaceutics 14(12):2589, 2022. https://pmc.ncbi.nlm.nih.gov/articles/PMC9786002/ (read 2026-11-14)
  • Mostafaei et al., alloy 625 water- and gas-atomised powders, Data in Brief 10:116-121, 2016. https://pmc.ncbi.nlm.nih.gov/articles/PMC5144650/ (read 2026-11-14)

Data: Binder jetting stage parameters reported in two metal studies

Compares printing, curing or drying, sintering and density parameters for binder-jetted H13 tool steel (Widomski et al., Materials 2025) and alloy 625 from water- and gas-atomised powders (Mostafaei et al., Data in Brief 2016). Values are as reported by each study for its own material and machine, and are not general settings.

Binder jetting stage parameters reported in two metal studies
Study caseLayer thickness (um)Drying or curing temperature (degC)Sintering temperature (degC)Sintering hold time (h)Sintering atmosphereHighest relative density reported (%)
H13 tool steel (Widomski et al. 2025)703513104Argon99.3
Alloy 625, water-atomised powder (Mostafaei et al. 2016)10017512704Vacuum95
Alloy 625, gas-atomised powder (Mostafaei et al. 2016)10017512854Vacuum99.2

Sources

Compiled by CASRAI from the sources above. Free to reuse under CC BY 4.0 with attribution.

Follow CASRAI

Research-administration guidance, standards updates and independent tool reviews.

Ask CASRAI · full access

Ask about Binder Jetting: How the Process Works and Its Limits

Full access: large monthly usage, up to 10 source passages behind each answer, and MCP and API access for Claude Code, Codex and other CLIs. Cancel any time.

An AI assistant for research: funder rules, compliance, methods and publishing. It links the sources behind its answers and labels answers that come from a web search.

Answers draw on CASRAI's guides and dictionary plus the federal and funder documents we index: Federal Register, Grants.gov, Regulations.gov and UKRI.

Works on this site and inside Claude, Cursor and the AI tools you already use.

Everything CASRAI publishes — this page, the dictionary, the guides and the news — stays open to read, with no account and no card.

Referenced across the research world

University of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logoUniversity of Cambridge logoColumbia University logoCrossref logoUniversity of Edinburgh logoHarvard University logoUniversity of Oxford logoPrinceton University logoStanford School of Medicine logoUniversity College London logoORCID logo
  • University of Cambridge logo
  • Columbia University logo
  • Crossref logo
  • University of Edinburgh logo
  • Harvard University logo
  • University of Oxford logo
  • Princeton University logo
  • Stanford School of Medicine logo
  • University College London logo
  • ORCID logo

View CASRAI adoption →